MechanicalAluminum 5052-H32Steel AISI 1045
Yield strength195MPa1producer-stated531MPa22.72x stronger
Ultimate tensile strength230MPa1producer-stated627MPa22.73x stronger
Elongation at break12%1in 2 in12%2
Young's modulus (stiffness)70GPa1210GPa33x stiffer
Density2,685kg/m³42.91x lighter7,800kg/m³3
Strength to weight72.6kN·m/kg7% higher68.1kN·m/kg
Stiffness to weight26.1MN·m/kg26.9MN·m/kg3% higher
Poisson's ratio0.3340.33
Shear modulus26.3GPa80.8GPa3.07x stiffer in shear
Bulk modulus68.6GPa175GPa2.55x higher
Speed of sound5,106m/s5,189m/s2% faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Steel AISI 1045
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Steel AISI 1045
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 5052-H32Steel AISI 1045
Thermal conductivitybase material138W/m·K140–45W/m·K3
Thermal expansion23.8µm/m·K112µm/m·K31.98x less
100 mm part over a 50 °C swing119µm growth60µm growth1.98x less
Specific heatat 100 °C963J/kg·K4460–480J/kg·K3
Heats up and cools (diffusivity)53.4mm²/s4.6x faster11.6mm²/s
Thermal shock resistance10,822W/m1.73x more resistant6,269W/m
Melting pointmelting range605–650°C1not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Steel AISI 1045
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Steel AISI 1045
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Kaiser Aluminum, Niagara LaSalle, Ovako, U.S. Department of Defense
Aluminum 5052-H32
5052-H32, Kaiser Aluminum tube & pipe typical datasheet (mechanical, CTE, melting); MIL-HDBK-5J (Poisson, density, specific heat)
Steel AISI 1045
AISI 1045 cold drawn bar (Niagara LaSalle) for mechanical; Ovako C45 (lists 'SAE 1045' as a similar designation) for physical constants
  1. 1
    Alloy 5052 Tube & Pipe Technical DataKaiser Aluminumarchived copyAluminum 5052-H32 · Yield strength: typical, 0.2% offsetAluminum 5052-H32 · Ultimate tensile strength: typicalAluminum 5052-H32 · Elongation at break: typicalAluminum 5052-H32 · Young's modulus (stiffness): typicalAluminum 5052-H32 · Thermal conductivity: base material: 5052 in O temper (same alloy, annealed); Kaiser typicalAluminum 5052-H32 · Thermal expansion: typical, mean 20-100 °CAluminum 5052-H32 · Melting point: melting range
  2. 2
    1045 PropertiesNiagara LaSallearchived copySteel AISI 1045 · Yield strength: producer-stated, cold drawnSteel AISI 1045 · Ultimate tensile strength: producer-stated, cold drawnSteel AISI 1045 · Elongation at break: in 2 in (50.8 mm)
  3. 3
    C45 Steel GradeOvakoSteel AISI 1045 · Young's modulus (stiffness): typicalSteel AISI 1045 · Density: typicalSteel AISI 1045 · Poisson's ratio: typicalSteel AISI 1045 · Thermal conductivity: typical range, ambientSteel AISI 1045 · Thermal expansion: typical, mean 20-300 °CSteel AISI 1045 · Specific heat: typical range, 50/100 °C
  4. 4
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 5052-H32 · Density: nominalAluminum 5052-H32 · Poisson's ratio: typical (handbook physical constant)Aluminum 5052-H32 · Specific heat: at 100 °C (212 °F); table covers O, H32, H34, H36, H38

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 5052-H32 stronger than Steel AISI 1045?

Steel AISI 1045 is stronger: its yield strength is 531 MPa against 195 MPa for Aluminum 5052-H32 (2.72x).

Which is lighter, Aluminum 5052-H32 or Steel AISI 1045?

Aluminum 5052-H32 is lighter: 2,685 kg/m³ against 7,800 kg/m³ for Steel AISI 1045.

Which is stiffer, Aluminum 5052-H32 or Steel AISI 1045?

Steel AISI 1045 is stiffer: Young's modulus 210 GPa against 70 GPa for Aluminum 5052-H32, so the same part in Steel AISI 1045 deflects less under the same load.

Which is lighter for the same job, Aluminum 5052-H32 or Steel AISI 1045?

For the same stiffness or strength: Aluminum 5052-H32 is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate; Steel AISI 1045 is lighter for a stiff rod or tie (tension).

Part that must beAluminum 5052-H32Steel AISI 1045
Stiff rod or tie (tension)3% heavierlighter
Stiff beam (bending)lighter1.68x heavier
Stiff panel or platelighter2.01x heavier
Strong rod or tielighter7% heavier
Strong beamlighter49% heavier
Strong panel or platelighter1.76x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Thermal

Which conducts heat better, Aluminum 5052-H32 or Steel AISI 1045?

Aluminum 5052-H32 conducts heat better: 138 W/m·K against 42.5 W/m·K for Steel AISI 1045.

Which expands less with temperature?

Steel AISI 1045 expands less: 12 µm/m·K against 23.8 µm/m·K for Aluminum 5052-H32.

Related comparisons