Materials / Compare

Aluminum 6061-T6 vs. Titanium Ti-6Al-4V

Compare Aluminum 6061-T6 vs. Titanium Ti-6Al-4V strength, stiffness, weight and thermal properties.

Aluminum 6061-T6Wrought
Titanium Ti-6Al-4VWrought
MechanicalAluminum 6061-T6Titanium Ti-6Al-4V
Yield strength276MPa1885MPa23.21x stronger
Ultimate tensile strength310MPa1940MPa23.03x stronger
Elongation at break17%116%2
Young's modulus (stiffness)68.3GPa1107–122GPa3
Density2,700kg/m³11.64x lighter4,430kg/m³2
Strength to weight102kN·m/kg200kN·m/kg1.95x higher
Stiffness to weight25.3MN·m/kg25.8MN·m/kg2% higher
Poisson's ratio0.3340.3422
Shear modulus25.7GPa42.7GPa1.66x stiffer in shear
Bulk modulus67GPa121GPa1.8x higher
Speed of sound5,030m/s5,084m/s1% faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6Titanium Ti-6Al-4V
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6Titanium Ti-6Al-4V
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 6061-T6Titanium Ti-6Al-4V
Thermal conductivity167W/m·K125.3x more heat through a fin6.6W/m·K3
Thermal expansion23.6µm/m·K19µm/m·K32.62x less
100 mm part over a 50 °C swing118µm growth45µm growth2.62x less
Specific heat896J/kg·K11.54x higher580J/kg·K3
Heats up and cools (diffusivity)69mm²/s26.9x faster2.57mm²/s
Thermal shock resistance19,159W/m5.14x more resistant3,730W/m
Melting pointsolidus-liquidus582–652°C1melting range1,630–1,650°C2
Max service temperaturenot sourced400°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6Titanium Ti-6Al-4V
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6Titanium Ti-6Al-4V
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Kaiser Aluminum, TIMET, U.S. Department of Defense
Aluminum 6061-T6
6061-T6/T651, Kaiser Aluminum typical properties; Poisson from MIL-HDBK-5J
Titanium Ti-6Al-4V
TIMETAL 6-4 (Ti-6Al-4V Grade 5) annealed plate typical (TIMET properties manual) + TIMET datasheet TMC-0150 physical properties
  1. 1
    Alloy 6061 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 6061-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 6061-T6 · Ultimate tensile strength: typicalAluminum 6061-T6 · Elongation at break: typical, in 4D, 0.500 in dia specimenAluminum 6061-T6 · Young's modulus (stiffness): typicalAluminum 6061-T6 · Density: nominalAluminum 6061-T6 · Thermal conductivity: typical, 20 °CAluminum 6061-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 6061-T6 · Specific heat: typical, at 100 °CAluminum 6061-T6 · Melting point: solidus-liquidus
  2. 2
    TIMETAL 6-4 PropertiesTIMETarchived copyTitanium Ti-6Al-4V · Yield strength: typical, plate (>0.187 in), annealed, 0.2% offsetTitanium Ti-6Al-4V · Ultimate tensile strength: typical, plate, annealedTitanium Ti-6Al-4V · Elongation at break: typical, in 2 in., plate annealedTitanium Ti-6Al-4V · Density: nominalTitanium Ti-6Al-4V · Poisson's ratio: mean of TIMET measurementsTitanium Ti-6Al-4V · Melting point: melting rangeTitanium Ti-6Al-4V · Max service temperature: upper recommended use temperature
  3. 3
    TIMETAL 6-4 Data SheetTIMETarchived copyTitanium Ti-6Al-4V · Young's modulus (stiffness): typical range, 20 °CTitanium Ti-6Al-4V · Thermal conductivity: typical, 20 °C, mill annealedTitanium Ti-6Al-4V · Thermal expansion: typical, mean 0-100 °CTitanium Ti-6Al-4V · Specific heat: typical, 20 °C
  4. 4
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 6061-T6 · Poisson's ratio: typical (handbook physical constant)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 6061-T6 stronger than Titanium Ti-6Al-4V?

Titanium Ti-6Al-4V is stronger: its yield strength is 885 MPa against 276 MPa for Aluminum 6061-T6 (3.21x).

Which is lighter, Aluminum 6061-T6 or Titanium Ti-6Al-4V?

Aluminum 6061-T6 is lighter: 2,700 kg/m³ against 4,430 kg/m³ for Titanium Ti-6Al-4V.

Which is stiffer, Aluminum 6061-T6 or Titanium Ti-6Al-4V?

Titanium Ti-6Al-4V is stiffer: Young's modulus 115 GPa against 68.3 GPa for Aluminum 6061-T6, so the same part in Titanium Ti-6Al-4V deflects less under the same load.

Which is lighter for the same job, Aluminum 6061-T6 or Titanium Ti-6Al-4V?

For the same stiffness or strength: Aluminum 6061-T6 is lighter for a stiff beam (bending), stiff panel or plate; Titanium Ti-6Al-4V is lighter for a stiff rod or tie (tension), strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 6061-T6Titanium Ti-6Al-4V
Stiff rod or tie (tension)2% heavierlighter
Stiff beam (bending)lighter27% heavier
Stiff panel or platelighter38% heavier
Strong rod or tie1.95x heavierlighter
Strong beam33% heavierlighter
Strong panel or plate9% heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Thermal

Which conducts heat better, Aluminum 6061-T6 or Titanium Ti-6Al-4V?

Aluminum 6061-T6 conducts heat better: 167 W/m·K against 6.6 W/m·K for Titanium Ti-6Al-4V.

Which expands less with temperature?

Titanium Ti-6Al-4V expands less: 9 µm/m·K against 23.6 µm/m·K for Aluminum 6061-T6.

Related comparisons