Materials / Compare

Aluminum 7075-T6 vs. DMLS 17-4PH Stainless Steel

Compare Aluminum 7075-T6 vs. DMLS 17-4PH Stainless Steel strength, stiffness, weight and thermal properties.

Aluminum 7075-T6Wrought
DMLS 17-4PH Stainless Steel3D printed metal (DMLS)
MechanicalAluminum 7075-T6DMLS 17-4PH Stainless Steel
Yield strength503MPa1mean861MPa21.71x stronger
Ultimate tensile strength572MPa1mean886MPa21.55x stronger
Elongation at break11%1mean at break19.9%21.81x more ductile
Young's modulus (stiffness)71GPa1base material197GPa32.77x stiffer
Density2,800kg/m³42.78x lightermean part density7,790kg/m³2
Strength to weight180kN·m/kg1.63x higher110kN·m/kg
Stiffness to weight25.4MN·m/kg25.3MN·m/kg
Poisson's ratio0.335base material0.2723
Shear modulus26.7GPa77.4GPa2.9x stiffer in shear
Bulk modulus69.6GPa144GPa2.07x higher
Speed of sound5,036m/s5,029m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6DMLS 17-4PH Stainless Steel
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6DMLS 17-4PH Stainless Steel
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 7075-T6DMLS 17-4PH Stainless Steel
Thermal conductivity130W/m·K47.26x more heat through a finbase material17.9W/m·K3
Thermal expansion23.4µm/m·K4mean 25-100 °C10.4µm/m·K22.25x less
100 mm part over a 50 °C swing117µm growth52µm growth2.25x less
Specific heat960J/kg·K42.09x higherbase material460J/kg·K3
Heats up and cools (diffusivity)48.4mm²/s9.68x faster5mm²/s
Thermal shock resistance26,370W/m4.82x more resistant5,474W/m
Melting pointmelting range532–635°C4not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6DMLS 17-4PH Stainless Steel
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6DMLS 17-4PH Stainless Steel
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: Kaiser Aluminum, EOS GmbH, Cleveland-Cliffs, U.S. Department of Defense
Aluminum 7075-T6
7075-T6/T651, Kaiser Aluminum rod & bar (mechanical) and sheet/coil/plate (physical) typical datasheets; Poisson from MIL-HDBK-5J
DMLS 17-4PH Stainless Steel
EOS StainlessSteel 17-4PH IndustryLine (powder 9011-0041), EOS M 290, 40 µm, default job 17-4PH_040_StainlessM291_100, as built, horizontal; ISO 6892 & ASTM E8M
  1. 1
    Alloy 7075 Rod & Bar Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 7075-T6 · Ultimate tensile strength: typicalAluminum 7075-T6 · Elongation at break: typical, in 4DAluminum 7075-T6 · Young's modulus (stiffness): typical
  2. 2
    EOS StainlessSteel 17-4PH IndustryLine Material Data Sheet, M 290EOS GmbHarchived copyDMLS 17-4PH Stainless Steel · Yield strength: mean, as built, horizontal (N=72)DMLS 17-4PH Stainless Steel · Ultimate tensile strength: mean, as built, horizontal (N=72)DMLS 17-4PH Stainless Steel · Elongation at break: mean at break, as built, horizontalDMLS 17-4PH Stainless Steel · Density: mean part density (ISO 3369)DMLS 17-4PH Stainless Steel · Thermal expansion: mean 25-100 °C, ASTM E228, AFTER atmospheric heat treatment (as-built value not published)
  3. 3
    17-4 PH Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsDMLS 17-4PH Stainless Steel · Young's modulus (stiffness): base material: wrought 17-4 PH, Condition H 900 (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Poisson's ratio: base material: wrought 17-4 PH, all conditions (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Thermal conductivity: base material: wrought 17-4 PH, Condition H 900, at 149 °C (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Specific heat: base material: wrought 17-4 PH, Condition A, 0-100 °C (Cleveland-Cliffs)
  4. 4
    Alloy 7075 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Density: nominalAluminum 7075-T6 · Thermal conductivity: typical, 20 °C, T651Aluminum 7075-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 7075-T6 · Specific heat: typical, at 100 °CAluminum 7075-T6 · Melting point: melting range
  5. 5
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 7075-T6 · Poisson's ratio: typical (handbook physical constant)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

DMLS 17-4PH Stainless Steel is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Aluminum 7075-T6 stronger than DMLS 17-4PH Stainless Steel?

DMLS 17-4PH Stainless Steel is stronger: its yield strength is 861 MPa against 503 MPa for Aluminum 7075-T6 (1.71x).

Which is lighter, Aluminum 7075-T6 or DMLS 17-4PH Stainless Steel?

Aluminum 7075-T6 is lighter: 2,800 kg/m³ against 7,790 kg/m³ for DMLS 17-4PH Stainless Steel.

Which is stiffer, Aluminum 7075-T6 or DMLS 17-4PH Stainless Steel?

DMLS 17-4PH Stainless Steel is stiffer: Young's modulus 197 GPa against 71 GPa for Aluminum 7075-T6, so the same part in DMLS 17-4PH Stainless Steel deflects less under the same load.

Which is lighter for the same job, Aluminum 7075-T6 or DMLS 17-4PH Stainless Steel?

For the same stiffness or strength: Aluminum 7075-T6 is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 7075-T6DMLS 17-4PH Stainless Steel
Stiff rod or tie (tension)about equalabout equal
Stiff beam (bending)lighter1.67x heavier
Stiff panel or platelighter1.98x heavier
Strong rod or tielighter1.63x heavier
Strong beamlighter1.94x heavier
Strong panel or platelighter2.13x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 7075-T6 or DMLS 17-4PH Stainless Steel?

DMLS 17-4PH Stainless Steel stretches further before it breaks: 19.9% elongation at break against 11% for Aluminum 7075-T6.

Thermal

Which conducts heat better, Aluminum 7075-T6 or DMLS 17-4PH Stainless Steel?

Aluminum 7075-T6 conducts heat better: 130 W/m·K against 17.9 W/m·K for DMLS 17-4PH Stainless Steel.

Which expands less with temperature?

DMLS 17-4PH Stainless Steel expands less: 10.4 µm/m·K against 23.4 µm/m·K for Aluminum 7075-T6.

Related comparisons