Materials / Compare

Aluminum 7075-T6 vs. Plastic HDPE

Compare Aluminum 7075-T6 vs. Plastic HDPE strength, stiffness, weight and thermal properties.

Aluminum 7075-T6Wrought
Plastic HDPEBulk polymer (molded or machined)
MechanicalAluminum 7075-T6Plastic HDPE
Yield strength503MPa121x stronger24MPa2
Ultimate tensile strength572MPa1not stated (yield given)
Elongation at break11%1not sourced
Young's modulus (stiffness)71GPa178.9x stiffer0.9GPa2
Density2,800kg/m³3950kg/m³22.95x lighter
Strength to weight180kN·m/kg7.11x higher25.3kN·m/kg
Stiffness to weight25.4MN·m/kg26.8x higher0.947MN·m/kg
Poisson's ratio0.334base material0.4–0.455
Shear modulus26.7GPa84.5x stiffer in shear0.316GPa
Bulk modulus69.6GPa34.8x higher2GPa
Speed of sound5,036m/s5.17x faster973m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6Plastic HDPE
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6Plastic HDPE
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 7075-T6Plastic HDPE
Thermal conductivity130W/m·K3base material0.4–0.49W/m·K5
Thermal expansion23.4µm/m·K35.13x lessbase material120µm/m·K5
100 mm part over a 50 °C swing117µm growth5.13x less600µm growth
Specific heat960J/kg·K3base material2,250J/kg·K52.34x higher
Heats up and cools (diffusivity)48.4mm²/s232x faster0.208mm²/s
Thermal shock resistance26,370W/m464x more resistant56.9W/m
Melting pointmelting range532–635°C3not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6Plastic HDPE
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6Plastic HDPE
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: Kaiser Aluminum, LyondellBasell, U.S. Department of Defense, INEOS Olefins & Polymers USA
Aluminum 7075-T6
7075-T6/T651, Kaiser Aluminum rod & bar (mechanical) and sheet/coil/plate (physical) typical datasheets; Poisson from MIL-HDBK-5J
Plastic HDPE
LyondellBasell Hostalen 23050 B high density polyethylene, typical ISO values
  1. 1
    Alloy 7075 Rod & Bar Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 7075-T6 · Ultimate tensile strength: typicalAluminum 7075-T6 · Elongation at break: typical, in 4DAluminum 7075-T6 · Young's modulus (stiffness): typical
  2. 2
    Hostalen 23050 B Product DataLyondellBasellPlastic HDPE · Yield strength: typical, tensile stress at yield 23 °C, 50 mm/min ISO 527Plastic HDPE · Young's modulus (stiffness): typical, tensile modulus 23 °C ISO 527Plastic HDPE · Density: typical, ISO 1183
  3. 3
    Alloy 7075 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Density: nominalAluminum 7075-T6 · Thermal conductivity: typical, 20 °C, T651Aluminum 7075-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 7075-T6 · Specific heat: typical, at 100 °CAluminum 7075-T6 · Melting point: melting range
  4. 4
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 7075-T6 · Poisson's ratio: typical (handbook physical constant)
  5. 5
    Typical Engineering Properties of High Density PolyethyleneINEOS Olefins & Polymers USAarchived copyPlastic HDPE · Poisson's ratio: base material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)Plastic HDPE · Thermal conductivity: base material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)Plastic HDPE · Thermal expansion: base material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)Plastic HDPE · Specific heat: base material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 7075-T6 stronger than Plastic HDPE?

Aluminum 7075-T6 is stronger: its yield strength is 503 MPa against 24 MPa for Plastic HDPE (21x).

Which is lighter, Aluminum 7075-T6 or Plastic HDPE?

Plastic HDPE is lighter: 950 kg/m³ against 2,800 kg/m³ for Aluminum 7075-T6.

Which is stiffer, Aluminum 7075-T6 or Plastic HDPE?

Aluminum 7075-T6 is stiffer: Young's modulus 71 GPa against 0.9 GPa for Plastic HDPE, so the same part in Aluminum 7075-T6 deflects less under the same load.

Which is lighter for the same job, Aluminum 7075-T6 or Plastic HDPE?

For the same stiffness or strength: Aluminum 7075-T6 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 7075-T6Plastic HDPE
Stiff rod or tie (tension)lighter26.8x heavier
Stiff beam (bending)lighter3.01x heavier
Stiff panel or platelighter46% heavier
Strong rod or tielighter7.11x heavier
Strong beamlighter2.58x heavier
Strong panel or platelighter1.55x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Thermal

Which conducts heat better, Aluminum 7075-T6 or Plastic HDPE?

Aluminum 7075-T6 conducts heat better: 130 W/m·K against 0.445 W/m·K for Plastic HDPE.

Which expands less with temperature?

Aluminum 7075-T6 expands less: 23.4 µm/m·K against 120 µm/m·K for Plastic HDPE.

Related comparisons