Materials / Plastic

Plastic HDPE

Plastic HDPE strength, stiffness, density and thermal properties, with their source.

A bracket in Plastic HDPE, smooth finish.

ProcessBulk polymer (molded or machined)
Mechanical
Yield strength24MPasourcetypical, tensile stress at yield 23 °C, 50 mm/min ISO 527
Ultimate tensile strengthnot sourced
Elongation at breaknot sourced
Young's modulus (stiffness)0.9GPasourcetypical, tensile modulus 23 °C ISO 527
Density950kg/m³sourcetypical, ISO 1183
Strength to weight25.3kN·m/kg
Stiffness to weight0.947MN·m/kg
Poisson's ratio0.4–0.45sourcebase material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)
Shear modulus0.316GPa
Bulk modulus2GPa
Speed of sound973m/s
Thermal
Thermal conductivity0.4–0.49W/m·Ksourcebase material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)
Thermal expansion120µm/m·Ksourcebase material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)
100 mm part over a 50 °C swing600µm growth
Specific heat2,250J/kg·Ksourcebase material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)
Heats up and cools (diffusivity)0.208mm²/s
Thermal shock resistance56.9W/m
Values forLyondellBasell Hostalen 23050 B high density polyethylene, typical ISO values

Among 72 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic HDPE
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic HDPE
Strength against density

Compare Plastic HDPE with