Materials / Compare

Aluminum 7075-T6 vs. Stainless Steel 17-4PH

Compare Aluminum 7075-T6 vs. Stainless Steel 17-4PH strength, stiffness, weight and thermal properties.

Aluminum 7075-T6Wrought
Stainless Steel 17-4PHWrought
MechanicalAluminum 7075-T6Stainless Steel 17-4PH
Yield strength503MPa11,275MPa22.53x stronger
Ultimate tensile strength572MPa11,379MPa22.41x stronger
Elongation at break11%122% more ductile9%2
Young's modulus (stiffness)71GPa1H 900197GPa22.77x stiffer
Density2,800kg/m³32.79x lighterH 9007,800kg/m³2
Strength to weight180kN·m/kg10% higher163kN·m/kg
Stiffness to weight25.4MN·m/kg25.3MN·m/kg
Poisson's ratio0.334H 9000.2722
Shear modulus26.7GPa77.4GPa2.9x stiffer in shear
Bulk modulus69.6GPa144GPa2.07x higher
Speed of sound5,036m/s5,026m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6Stainless Steel 17-4PH
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6Stainless Steel 17-4PH
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 7075-T6Stainless Steel 17-4PH
Thermal conductivity130W/m·K37.26x more heat through a finat 149 °C17.9W/m·K2
Thermal expansion23.4µm/m·K3mean10.8µm/m·K22.17x less
100 mm part over a 50 °C swing117µm growth54µm growth2.17x less
Specific heat960J/kg·K32.09x highermean460J/kg·K2
Heats up and cools (diffusivity)48.4mm²/s9.69x faster4.99mm²/s
Thermal shock resistance26,370W/m3.38x more resistant7,809W/m
Melting pointmelting range532–635°C3not sourced
Max service temperaturenot sourced316°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6Stainless Steel 17-4PH
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6Stainless Steel 17-4PH
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Kaiser Aluminum, Cleveland-Cliffs, U.S. Department of Defense
Aluminum 7075-T6
7075-T6/T651, Kaiser Aluminum rod & bar (mechanical) and sheet/coil/plate (physical) typical datasheets; Poisson from MIL-HDBK-5J
Stainless Steel 17-4PH
Cleveland-Cliffs 17-4 PH, Condition H 900, sheet/strip, transverse (Product Data Bulletin, May 2021)
  1. 1
    Alloy 7075 Rod & Bar Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 7075-T6 · Ultimate tensile strength: typicalAluminum 7075-T6 · Elongation at break: typical, in 4DAluminum 7075-T6 · Young's modulus (stiffness): typical
  2. 2
    17-4 PH Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsStainless Steel 17-4PH · Yield strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Ultimate tensile strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Elongation at break: typical, transverse, in 2 in. (50.8 mm)Stainless Steel 17-4PH · Young's modulus (stiffness): H 900Stainless Steel 17-4PH · Density: H 900Stainless Steel 17-4PH · Poisson's ratio: H 900 (column)Stainless Steel 17-4PH · Thermal conductivity: at 149 °C (300 °F), H 900Stainless Steel 17-4PH · Thermal expansion: mean, 21–93 °C (70–200 °F), H 900Stainless Steel 17-4PH · Specific heat: mean, 0–100 °C, H 900Stainless Steel 17-4PH · Max service temperature: strength-retention limit (not oxidation)
  3. 3
    Alloy 7075 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Density: nominalAluminum 7075-T6 · Thermal conductivity: typical, 20 °C, T651Aluminum 7075-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 7075-T6 · Specific heat: typical, at 100 °CAluminum 7075-T6 · Melting point: melting range
  4. 4
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 7075-T6 · Poisson's ratio: typical (handbook physical constant)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 7075-T6 stronger than Stainless Steel 17-4PH?

Stainless Steel 17-4PH is stronger: its yield strength is 1,275 MPa against 503 MPa for Aluminum 7075-T6 (2.53x).

Which is lighter, Aluminum 7075-T6 or Stainless Steel 17-4PH?

Aluminum 7075-T6 is lighter: 2,800 kg/m³ against 7,800 kg/m³ for Stainless Steel 17-4PH.

Which is stiffer, Aluminum 7075-T6 or Stainless Steel 17-4PH?

Stainless Steel 17-4PH is stiffer: Young's modulus 197 GPa against 71 GPa for Aluminum 7075-T6, so the same part in Stainless Steel 17-4PH deflects less under the same load.

Which is lighter for the same job, Aluminum 7075-T6 or Stainless Steel 17-4PH?

For the same stiffness or strength: Aluminum 7075-T6 is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 7075-T6Stainless Steel 17-4PH
Stiff rod or tie (tension)about equalabout equal
Stiff beam (bending)lighter1.67x heavier
Stiff panel or platelighter1.98x heavier
Strong rod or tielighter10% heavier
Strong beamlighter50% heavier
Strong panel or platelighter1.75x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 7075-T6 or Stainless Steel 17-4PH?

Aluminum 7075-T6 stretches further before it breaks: 11% elongation at break against 9% for Stainless Steel 17-4PH.

Thermal

Which conducts heat better, Aluminum 7075-T6 or Stainless Steel 17-4PH?

Aluminum 7075-T6 conducts heat better: 130 W/m·K against 17.9 W/m·K for Stainless Steel 17-4PH.

Which expands less with temperature?

Stainless Steel 17-4PH expands less: 10.8 µm/m·K against 23.4 µm/m·K for Aluminum 7075-T6.

Related comparisons