Stainless Steel 17-4PH (H900) strength, stiffness, density and thermal properties, with their source.

A bracket in Stainless Steel 17-4PH, brushed finish.

ProcessWrought
Mechanical
Yield strength1,275MPasourcetypical, transverse, sheet/strip
Ultimate tensile strength1,379MPasourcetypical, transverse, sheet/strip
Elongation at break9%sourcetypical, transverse, in 2 in. (50.8 mm)
Young's modulus (stiffness)197GPasourceH 900
Density7,800kg/m³sourceH 900
Strength to weight163kN·m/kg
Stiffness to weight25.3MN·m/kg
Poisson's ratio0.272sourceH 900 (column)
Shear modulus77.4GPa
Bulk modulus144GPa
Speed of sound5,026m/s
Thermal
Thermal conductivity17.9W/m·Ksourceat 149 °C (300 °F), H 900
Thermal expansion10.8µm/m·Ksourcemean, 21–93 °C (70–200 °F), H 900
100 mm part over a 50 °C swing54µm growth
Specific heat460J/kg·Ksourcemean, 0–100 °C, H 900
Heats up and cools (diffusivity)4.99mm²/s
Thermal shock resistance7,809W/m
Max service temperature316°Csourcestrength-retention limit (not oxidation)
Values forCleveland-Cliffs 17-4 PH, Condition H 900, sheet/strip, transverse (Product Data Bulletin, May 2021)

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelStainless Steel 17-4PH
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickStainless Steel 17-4PH
Strength against density