Mechanical
Yield strength503MPasourcetypical, 0.2% offset, .500 in dia specimen221MPasourcetypical
Ultimate tensile strength572MPasourcetypical2.02x stronger283MPasourcetypical
Elongation at break11%sourcetypical, in 4D10%sourcetypical, in 2 in.
Young's modulus (stiffness)71GPasourcetypical85.5GPasourcetypical20% stiffer
Density2,800kg/m³sourcenominal6,600kg/m³sourcetypical
Strength to weight180kN·m/kg5.36x higher33.5kN·m/kg
Stiffness to weight25.4MN·m/kg1.96x higher13MN·m/kg
Poisson's ratio0.33sourcetypical (handbook physical constant)0.27sourcetypical, Zamak 3 hot-chamber die cast
Shear modulus26.7GPa33.7GPa26% stiffer in shear
Bulk modulus69.6GPa62GPa
Speed of sound5,036m/s3,599m/s
Thermal
Thermal conductivity130W/m·Ksourcetypical, 20 °C, T651113W/m·Ksourcetypical
Thermal expansion23.4µm/m·Ksourcetypical, mean 20-100 °C27.4µm/m·Ksourcetypical
100 mm part over a 50 °C swing117µm growth17% less137µm growth
Specific heat960J/kg·Ksourcetypical, at 100 °C419J/kg·Ksourcetypical
Heats up and cools (diffusivity)48.4mm²/s18% faster40.9mm²/s
Thermal shock resistance26,370W/m3.39x more resistant7,782W/m
Melting point532–635°Csourcemelting range381–387°Csourcemelting range
Values for7075-T6/T651, Kaiser Aluminum rod & bar (mechanical) and sheet/coil/plate (physical) typical datasheets; Poisson from MIL-HDBK-5JZamak 3 (ASTM B86 die cast), Nathan Trotter (zinc alloy producer) technical data sheet, typical values

Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Is Aluminum 7075-T6 stronger than Zinc Zamak 3?

Aluminum 7075-T6 is stronger: its yield strength is 503 MPa against 221 MPa for Zinc Zamak 3 (2.28x).

Which is lighter, Aluminum 7075-T6 or Zinc Zamak 3?

Aluminum 7075-T6 is lighter: 2,800 kg/m³ against 6,600 kg/m³ for Zinc Zamak 3.

Which is stiffer, Aluminum 7075-T6 or Zinc Zamak 3?

Zinc Zamak 3 is stiffer: Young's modulus 85.5 GPa against 71 GPa for Aluminum 7075-T6, so the same part in Zinc Zamak 3 deflects less under the same load.

Which is lighter for the same job, Aluminum 7075-T6 or Zinc Zamak 3?

For the same stiffness or strength: Aluminum 7075-T6 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 7075-T6Zinc Zamak 3
Stiff rod or tie (tension)lighter1.96x heavier
Stiff beam (bending)lighter2.15x heavier
Stiff panel or platelighter2.22x heavier
Strong rod or tielighter5.36x heavier
Strong beamlighter4.08x heavier
Strong panel or platelighter3.56x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which conducts heat better, Aluminum 7075-T6 or Zinc Zamak 3?

Aluminum 7075-T6 conducts heat better: 130 W/m·K against 113 W/m·K for Zinc Zamak 3.

Which expands less with temperature?

Aluminum 7075-T6 expands less: 23.4 µm/m·K against 27.4 µm/m·K for Zinc Zamak 3.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelAluminum 7075-T6Zinc Zamak 3
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickAluminum 7075-T6Zinc Zamak 3
Strength against density

Related comparisons