Thermal conductivity against densityHigher and further left: spreads more heat for its weightThermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browser
Sources4 documents: Kaiser Aluminum, EOS GmbH, Cleveland-Cliffs, U.S. Department of Defense
Aluminum
6061-T6/T651, Kaiser Aluminum typical properties (sheet, coil & plate datasheet); Poisson from MIL-HDBK-5J
DMLS 17-4PH Stainless Steel
EOS StainlessSteel 17-4PH IndustryLine (powder 9011-0041), EOS M 290, 40 µm, default job 17-4PH_040_StainlessM291_100, as built, horizontal; ISO 6892 & ASTM E8M
1
Alloy 6061 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum · Ultimate tensile strength: typicalAluminum · Elongation at break: typical, in 4D, 0.500 in dia specimenAluminum · Young's modulus (stiffness): typicalAluminum · Density: nominalAluminum · Thermal conductivity: typical, 20 °CAluminum · Thermal expansion: typical, mean 20-100 °CAluminum · Specific heat: typical, at 100 °CAluminum · Melting point: solidus-liquidus
2
EOS StainlessSteel 17-4PH IndustryLine Material Data Sheet, M 290EOS GmbHarchived copyDMLS 17-4PH Stainless Steel · Yield strength: mean, as built, horizontal (N=72)DMLS 17-4PH Stainless Steel · Ultimate tensile strength: mean, as built, horizontal (N=72)DMLS 17-4PH Stainless Steel · Elongation at break: mean at break, as built, horizontalDMLS 17-4PH Stainless Steel · Density: mean part density (ISO 3369)DMLS 17-4PH Stainless Steel · Thermal expansion: mean 25-100 °C, ASTM E228, AFTER atmospheric heat treatment (as-built value not published)
3
17-4 PH Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsDMLS 17-4PH Stainless Steel · Young's modulus (stiffness): base material: wrought 17-4 PH, Condition H 900 (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Poisson's ratio: base material: wrought 17-4 PH, all conditions (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Thermal conductivity: base material: wrought 17-4 PH, Condition H 900, at 149 °C (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Specific heat: base material: wrought 17-4 PH, Condition A, 0-100 °C (Cleveland-Cliffs)
4
MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum · Poisson's ratio: typical (handbook physical constant)
Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
DMLS 17-4PH Stainless Steel is 3D printed: its properties depend on build direction and print settings; these are typical values.
Questions
Mechanical
Is Aluminum stronger than DMLS 17-4PH Stainless Steel?
DMLS 17-4PH Stainless Steel is stronger: its yield strength is 861 MPa against 276 MPa for Aluminum (3.12x).
Which is lighter, Aluminum or DMLS 17-4PH Stainless Steel?
Aluminum is lighter: 2,700 kg/m³ against 7,790 kg/m³ for DMLS 17-4PH Stainless Steel.
Which is stiffer, Aluminum or DMLS 17-4PH Stainless Steel?
DMLS 17-4PH Stainless Steel is stiffer: Young's modulus 197 GPa against 68.3 GPa for Aluminum, so the same part in DMLS 17-4PH Stainless Steel deflects less under the same load.
Which is lighter for the same job, Aluminum or DMLS 17-4PH Stainless Steel?
For the same stiffness or strength: Aluminum is lighter for a stiff beam (bending), stiff panel or plate, strong beam, strong panel or plate; DMLS 17-4PH Stainless Steel is lighter for a strong rod or tie.
Part that must be
Aluminum
DMLS 17-4PH Stainless Steel
Stiff rod or tie (tension)
about equal
about equal
Stiff beam (bending)
lighter
1.7x heavier
Stiff panel or plate
lighter
2.03x heavier
Strong rod or tie
8% heavier
lighter
Strong beam
lighter
35% heavier
Strong panel or plate
lighter
1.63x heavier
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Which is more ductile, Aluminum or DMLS 17-4PH Stainless Steel?
DMLS 17-4PH Stainless Steel stretches further before it breaks: 19.9% elongation at break against 17% for Aluminum.
Thermal
Which conducts heat better, Aluminum or DMLS 17-4PH Stainless Steel?
Aluminum conducts heat better: 167 W/m·K against 17.9 W/m·K for DMLS 17-4PH Stainless Steel.
Which expands less with temperature?
DMLS 17-4PH Stainless Steel expands less: 10.4 µm/m·K against 23.6 µm/m·K for Aluminum.