Thermal conductivity against densityHigher and further left: spreads more heat for its weightThermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browser
Sources7 documents: Kaiser Aluminum, EOS GmbH, U.S. Department of Defense, Steel Construction Institute, Cleveland-Cliffs
Aluminum
6061-T6/T651, Kaiser Aluminum typical properties (sheet, coil & plate datasheet); Poisson from MIL-HDBK-5J
DMLS 316L Stainless Steel
EOS StainlessSteel 316L (powder 9011-0032), EOS M 290, ParameterSet 316L 20µm Surface M290/400W, as manufactured, horizontal; ISO 6892-1
1
Alloy 6061 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum · Ultimate tensile strength: typicalAluminum · Elongation at break: typical, in 4D, 0.500 in dia specimenAluminum · Young's modulus (stiffness): typicalAluminum · Density: nominalAluminum · Thermal conductivity: typical, 20 °CAluminum · Thermal expansion: typical, mean 20-100 °CAluminum · Specific heat: typical, at 100 °CAluminum · Melting point: solidus-liquidus
2
EOS StainlessSteel 316L Material Data SheetEOS GmbHarchived copyDMLS 316L Stainless Steel · Yield strength: typical, as manufactured, horizontalDMLS 316L Stainless Steel · Ultimate tensile strength: typical, as manufactured, horizontalDMLS 316L Stainless Steel · Elongation at break: typical at break, as manufactured, horizontalDMLS 316L Stainless Steel · Thermal expansion: mean 25-100 °C, ASTM E228
3
EOS StainlessSteel 316L Material Data Sheet, M 280 and M 290 (2014)EOS GmbHarchived copyDMLS 316L Stainless Steel · Young's modulus (stiffness): typical, as built, horizontal (XY); EOSINT M280-400W / M290-400W, 316L_Surface 1.0, 20 µm (2014 sheet)
4
EOS StainlessSteel 316L Material Data Sheet, FlexLine, M 290 (2016)EOS GmbHarchived copyDMLS 316L Stainless Steel · Density: part density (ISO 3369, not labelled min or typical), EOS M 290, 40 µm FlexLine
5
MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum · Poisson's ratio: typical (handbook physical constant)
6
Design Manual for Structural Stainless Steel, 4th Edition (P413)Steel Construction Institutearchived copyDMLS 316L Stainless Steel · Poisson's ratio: base material: austenitic stainless steels incl. 1.4404 (316L), design value
7
316/316L Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsDMLS 316L Stainless Steel · Thermal conductivity: base material: wrought 316/316L (Cleveland-Cliffs), at 100 °CDMLS 316L Stainless Steel · Specific heat: base material: wrought 316/316L (Cleveland-Cliffs), 0-100 °C
Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
DMLS 316L Stainless Steel is 3D printed: its properties depend on build direction and print settings; these are typical values.
Questions
Mechanical
Is Aluminum stronger than DMLS 316L Stainless Steel?
DMLS 316L Stainless Steel is stronger: its yield strength is 530 MPa against 276 MPa for Aluminum (1.92x).
Which is lighter, Aluminum or DMLS 316L Stainless Steel?
Aluminum is lighter: 2,700 kg/m³ against 7,900 kg/m³ for DMLS 316L Stainless Steel.
Which is stiffer, Aluminum or DMLS 316L Stainless Steel?
DMLS 316L Stainless Steel is stiffer: Young's modulus 185 GPa against 68.3 GPa for Aluminum, so the same part in DMLS 316L Stainless Steel deflects less under the same load.
Which is lighter for the same job, Aluminum or DMLS 316L Stainless Steel?
For the same stiffness or strength: Aluminum is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.
Part that must be
Aluminum
DMLS 316L Stainless Steel
Stiff rod or tie (tension)
lighter
8% heavier
Stiff beam (bending)
lighter
1.78x heavier
Stiff panel or plate
lighter
2.1x heavier
Strong rod or tie
lighter
1.52x heavier
Strong beam
lighter
1.89x heavier
Strong panel or plate
lighter
2.11x heavier
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Which is more ductile, Aluminum or DMLS 316L Stainless Steel?
DMLS 316L Stainless Steel stretches further before it breaks: 40% elongation at break against 17% for Aluminum.
Thermal
Which conducts heat better, Aluminum or DMLS 316L Stainless Steel?
Aluminum conducts heat better: 167 W/m·K against 16.2 W/m·K for DMLS 316L Stainless Steel.
Which expands less with temperature?
DMLS 316L Stainless Steel expands less: 15.7 µm/m·K against 23.6 µm/m·K for Aluminum.