Materials / Compare

Aluminum vs. Stainless Steel 17-4PH

Compare Aluminum vs. Stainless Steel 17-4PH strength, stiffness, weight and thermal properties.

AluminumWrought
Stainless Steel 17-4PHWrought
MechanicalAluminumStainless Steel 17-4PH
Yield strength276MPa11,275MPa24.62x stronger
Ultimate tensile strength310MPa11,379MPa24.45x stronger
Elongation at break17%11.89x more ductile9%2
Young's modulus (stiffness)68.3GPa1H 900197GPa22.88x stiffer
Density2,700kg/m³12.89x lighterH 9007,800kg/m³2
Strength to weight102kN·m/kg163kN·m/kg1.6x higher
Stiffness to weight25.3MN·m/kg25.3MN·m/kg
Poisson's ratio0.333H 9000.2722
Shear modulus25.7GPa77.4GPa3.02x stiffer in shear
Bulk modulus67GPa144GPa2.15x higher
Speed of sound5,030m/s5,026m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30AluminumStainless Steel 17-4PH
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30AluminumStainless Steel 17-4PH
Strength against densityHigher and further left: stronger for its weight
ThermalAluminumStainless Steel 17-4PH
Thermal conductivity167W/m·K19.33x more heat through a finat 149 °C17.9W/m·K2
Thermal expansion23.6µm/m·K1mean10.8µm/m·K22.19x less
100 mm part over a 50 °C swing118µm growth54µm growth2.19x less
Specific heat896J/kg·K11.95x highermean460J/kg·K2
Heats up and cools (diffusivity)69mm²/s13.8x faster4.99mm²/s
Thermal shock resistance19,159W/m2.45x more resistant7,809W/m
Melting pointsolidus-liquidus582–652°C1not sourced
Max service temperaturenot sourced316°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30AluminumStainless Steel 17-4PH
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30AluminumStainless Steel 17-4PH
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources3 documents: Kaiser Aluminum, Cleveland-Cliffs, U.S. Department of Defense
Aluminum
6061-T6/T651, Kaiser Aluminum typical properties (sheet, coil & plate datasheet); Poisson from MIL-HDBK-5J
Stainless Steel 17-4PH
Cleveland-Cliffs 17-4 PH, Condition H 900, sheet/strip, transverse (Product Data Bulletin, May 2021)
  1. 1
    Alloy 6061 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum · Ultimate tensile strength: typicalAluminum · Elongation at break: typical, in 4D, 0.500 in dia specimenAluminum · Young's modulus (stiffness): typicalAluminum · Density: nominalAluminum · Thermal conductivity: typical, 20 °CAluminum · Thermal expansion: typical, mean 20-100 °CAluminum · Specific heat: typical, at 100 °CAluminum · Melting point: solidus-liquidus
  2. 2
    17-4 PH Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsStainless Steel 17-4PH · Yield strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Ultimate tensile strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Elongation at break: typical, transverse, in 2 in. (50.8 mm)Stainless Steel 17-4PH · Young's modulus (stiffness): H 900Stainless Steel 17-4PH · Density: H 900Stainless Steel 17-4PH · Poisson's ratio: H 900 (column)Stainless Steel 17-4PH · Thermal conductivity: at 149 °C (300 °F), H 900Stainless Steel 17-4PH · Thermal expansion: mean, 21–93 °C (70–200 °F), H 900Stainless Steel 17-4PH · Specific heat: mean, 0–100 °C, H 900Stainless Steel 17-4PH · Max service temperature: strength-retention limit (not oxidation)
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum · Poisson's ratio: typical (handbook physical constant)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum stronger than Stainless Steel 17-4PH?

Stainless Steel 17-4PH is stronger: its yield strength is 1,275 MPa against 276 MPa for Aluminum (4.62x).

Which is lighter, Aluminum or Stainless Steel 17-4PH?

Aluminum is lighter: 2,700 kg/m³ against 7,800 kg/m³ for Stainless Steel 17-4PH.

Which is stiffer, Aluminum or Stainless Steel 17-4PH?

Stainless Steel 17-4PH is stiffer: Young's modulus 197 GPa against 68.3 GPa for Aluminum, so the same part in Stainless Steel 17-4PH deflects less under the same load.

Which is lighter for the same job, Aluminum or Stainless Steel 17-4PH?

For the same stiffness or strength: Aluminum is lighter for a stiff beam (bending), stiff panel or plate, strong beam, strong panel or plate; Stainless Steel 17-4PH is lighter for a strong rod or tie.

Part that must beAluminumStainless Steel 17-4PH
Stiff rod or tie (tension)about equalabout equal
Stiff beam (bending)lighter1.7x heavier
Stiff panel or platelighter2.03x heavier
Strong rod or tie1.6x heavierlighter
Strong beamlighter4% heavier
Strong panel or platelighter34% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum or Stainless Steel 17-4PH?

Aluminum stretches further before it breaks: 17% elongation at break against 9% for Stainless Steel 17-4PH.

Thermal

Which conducts heat better, Aluminum or Stainless Steel 17-4PH?

Aluminum conducts heat better: 167 W/m·K against 17.9 W/m·K for Stainless Steel 17-4PH.

Which expands less with temperature?

Stainless Steel 17-4PH expands less: 10.8 µm/m·K against 23.6 µm/m·K for Aluminum.