Materials / Compare

Concrete vs. FDM HIPS

Compare Concrete vs. FDM HIPS strength, stiffness, weight and thermal properties.

ConcreteCast
FDM HIPS3D printed (FDM)
MechanicalConcreteFDM HIPS
Yield strengthnone (brittle)not given (tensile used)
Ultimate tensile strengthnot sourced18.4MPa1
Compressive strength27.6MPa2not sourced
Flexural strengthnot sourced31.8MPa1
Elongation at breaknone (brittle)1.4%1
Young's modulus (stiffness)design value25.1GPa31.59GPa1
Density2,240–2,400kg/m³41,023kg/m³1
Strength to weightnot sourced18kN·m/kg
Stiffness to weight10.8MN·m/kg6.97x higher1.55MN·m/kg
Poisson's ratio0.15–0.25not sourced
Shear modulus10.7GPanot sourced
Bulk modulus12.9GPanot sourced
Speed of sound3,289m/s2.64x faster1,246m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30ConcreteFDM HIPS
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM HIPS
Strength against densityHigher and further left: stronger for its weight
ThermalConcreteFDM HIPS
Thermal conductivity0.9W/m·K65.29x more heat through a finbase material0.17W/m·K7
Thermal expansion8–12µm/m·K8base material80µm/m·K7
100 mm part over a 50 °C swing50µm growth8x less400µm growth
Specific heat900J/kg·K9not sourced
Heats up and cools (diffusivity)0.431mm²/snot sourced
Thermal shock resistancenot sourcednot sourced
Glass transitionnot sourced99°C1
Max service temperature65°C5HDT 1.8 MPa86°C1
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30ConcreteFDM HIPS
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30ConcreteFDM HIPS
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA sample part to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources9 documents: BASF Forward AM, National Ready Mixed Concrete Association, Federal Highway Administration, Oak Ridge National Laboratory, USDA Forest Products Laboratory, INEOS Styrolution, National Institute of Standards and Technology
Concrete
Normal-weight portland cement concrete, strength class f'c = 4000 psi (28 MPa) per NRMCA CIP 35; density NRMCA CIP 36; thermal conductivity USDA FPL Wood Handbook; service temperature ORNL/NRC review
FDM HIPS
BASF Forward AM (BASF 3D Printing Solutions) Ultrafuse HiPS, TDS v2.2 (13.11.2019), printed specimens, XY 'Flat'. Specimen print settings are not stated; recommended processing on the sheet: nozzle 240-260 °C, bed 100-120 °C, 40-80 mm/s. Product is discontinued (Forward AM product page) but the TDS is still served by Forward AM.
  1. 1
    Ultrafuse HiPS Technical Data Sheet, v2.2 (2019)BASF Forward AMarchived copyFDM HIPS · Ultimate tensile strength: typicalFDM HIPS · Flexural strength: typicalFDM HIPS · Elongation at break: typicalFDM HIPS · Young's modulus (stiffness): typicalFDM HIPS · Density: typicalFDM HIPS · Glass transition: typicalFDM HIPS · Max service temperature: HDT 1.8 MPa
  2. 2
    CIP 35: Testing Compressive Strength of ConcreteNational Ready Mixed Concrete Associationarchived copyConcrete · Compressive strength: specified compressive strength class (f'c), not a measured typical
  3. 3
    LRFD Steel Girder Superstructure Bridge Design Example, Design Step 2: Concrete Deck DesignFederal Highway AdministrationConcrete · Young's modulus (stiffness): design value: AASHTO LRFD 5.4.2.4 applied by FHWA to f'c = 4.0 ksi normal-weight concrete
  4. 4
    CIP 36: Structural Lightweight ConcreteNational Ready Mixed Concrete Associationarchived copyConcrete · Density: range for normalweight concrete
  5. 5
    The Effect of Elevated Temperature on Concrete Materials and Structures: A Literature Review (ORNL/TM-2005/553)Oak Ridge National Laboratoryarchived copyConcrete · Poisson's ratio: general range at normal ambient conditions (overall 0.11-0.32)Concrete · Max service temperature: code long-term temperature limit (ASME Code, concrete containments)
  6. 6
    Wood Handbook (FPL-GTR-282), Chapter 4: Moisture Relations and Physical Properties of WoodUSDA Forest Products LaboratoryConcrete · Thermal conductivity: typical (comparative value)
  7. 7
    Styrolution PS 486N (HIPS) Product Data SheetINEOS StyrolutionFDM HIPS · Thermal conductivity: base material: INEOS Styrolution PS 486N injection-molding HIPS, typicalFDM HIPS · Thermal expansion: base material: INEOS Styrolution PS 486N injection-molding HIPS, typical
  8. 8
    Thermal Coefficient of Portland Cement ConcreteFederal Highway AdministrationConcrete · Thermal expansion: typical range for portland cement concrete (aggregate dependent)
  9. 9
    Best Practice Guidelines for Structural Fire Resistance Design of Concrete and Steel Buildings (TN 1681)National Institute of Standards and Technologyarchived copyConcrete · Specific heat: typical (NIST guidance for thermal analysis)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

FDM HIPS is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Which is lighter, Concrete or FDM HIPS?

FDM HIPS is lighter: 1,023 kg/m³ against 2,320 kg/m³ for Concrete.

Which is stiffer, Concrete or FDM HIPS?

Concrete is stiffer: Young's modulus 25.1 GPa against 1.59 GPa for FDM HIPS, so the same part in Concrete deflects less under the same load.

Which is lighter for the same job, Concrete or FDM HIPS?

For the same stiffness or strength: Concrete is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate.

Part that must beConcreteFDM HIPS
Stiff rod or tie (tension)lighter6.97x heavier
Stiff beam (bending)lighter1.75x heavier
Stiff panel or platelighter11% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Thermal

Which conducts heat better, Concrete or FDM HIPS?

Concrete conducts heat better: 0.9 W/m·K against 0.17 W/m·K for FDM HIPS.

Which expands less with temperature?

Concrete expands less: 10 µm/m·K against 80 µm/m·K for FDM HIPS.

Related comparisons