Materials / Compare

Concrete vs. Plastic ABS

Compare Concrete vs. Plastic ABS strength, stiffness, weight and thermal properties.

ConcreteCast
Plastic ABS3D printed (FDM)
MechanicalConcretePlastic ABS
Yield strengthnone (brittle)38.1MPa1
Ultimate tensile strengthnot sourced38.1MPa1
Compressive strength27.6MPa2not sourced
Flexural strengthnot sourced61.1MPa1
Elongation at breaknone (brittle)4.6%1
Young's modulus (stiffness)design value25.1GPa31.96GPa1
Density2,240–2,400kg/m³41,100kg/m³1
Strength to weightnot sourced34.6kN·m/kg
Stiffness to weight10.8MN·m/kg6.07x higher1.78MN·m/kg
Poisson's ratio0.15–0.25base material0.396
Shear modulus10.7GPa15.1x stiffer in shear0.706GPa
Bulk modulus12.9GPa4.33x higher2.97GPa
Speed of sound3,289m/s2.46x faster1,336m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30ConcretePlastic ABS
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic ABS
Strength against densityHigher and further left: stronger for its weight
ThermalConcretePlastic ABS
Thermal conductivity0.9W/m·K75.29x more heat through a finbase material0.17W/m·K8
Thermal expansion8–12µm/m·K9base material80–110µm/m·K8
100 mm part over a 50 °C swing50µm growth9.5x less475µm growth
Specific heat900J/kg·K10not sourced
Heats up and cools (diffusivity)0.431mm²/snot sourced
Thermal shock resistancenot sourced21.2W/m
Glass transitionnot sourced101°C1
Max service temperature65°C5HDT 0.455 MPa86.6°C1
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30ConcretePlastic ABS
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30ConcretePlastic ABS
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA sample part to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources10 documents: UltiMaker, National Ready Mixed Concrete Association, Federal Highway Administration, Oak Ridge National Laboratory, Covestro, USDA Forest Products Laboratory, INEOS Styrolution, National Institute of Standards and Technology
Concrete
Normal-weight portland cement concrete, strength class f'c = 4000 psi (28 MPa) per NRMCA CIP 35; density NRMCA CIP 36; thermal conductivity USDA FPL Wood Handbook; service temperature ORNL/NRC review
Plastic ABS
Ultimaker ABS, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS v5.00, April 20, 2022.
  1. 1
    Ultimaker ABS Technical Data Sheet, v5.00UltiMakerarchived copyPlastic ABS · Yield strength: typicalPlastic ABS · Ultimate tensile strength: typical, peak stress (= stress at yield)Plastic ABS · Flexural strength: typicalPlastic ABS · Elongation at break: typicalPlastic ABS · Young's modulus (stiffness): typicalPlastic ABS · Density: typicalPlastic ABS · Glass transition: typicalPlastic ABS · Max service temperature: HDT 0.455 MPa (printed specimens)
  2. 2
    CIP 35: Testing Compressive Strength of ConcreteNational Ready Mixed Concrete Associationarchived copyConcrete · Compressive strength: specified compressive strength class (f'c), not a measured typical
  3. 3
    LRFD Steel Girder Superstructure Bridge Design Example, Design Step 2: Concrete Deck DesignFederal Highway AdministrationConcrete · Young's modulus (stiffness): design value: AASHTO LRFD 5.4.2.4 applied by FHWA to f'c = 4.0 ksi normal-weight concrete
  4. 4
    CIP 36: Structural Lightweight ConcreteNational Ready Mixed Concrete Associationarchived copyConcrete · Density: range for normalweight concrete
  5. 5
    The Effect of Elevated Temperature on Concrete Materials and Structures: A Literature Review (ORNL/TM-2005/553)Oak Ridge National Laboratoryarchived copyConcrete · Poisson's ratio: general range at normal ambient conditions (overall 0.11-0.32)Concrete · Max service temperature: code long-term temperature limit (ASME Code, concrete containments)
  6. 6
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroarchived copyPlastic ABS · Poisson's ratio: base material: ABS family typical (Covestro Part and Mold Design guide, Table 3-1)
  7. 7
    Wood Handbook (FPL-GTR-282), Chapter 4: Moisture Relations and Physical Properties of WoodUSDA Forest Products LaboratoryConcrete · Thermal conductivity: typical (comparative value)
  8. 8
    Terluran GP-22 (ABS) Product Data SheetINEOS StyrolutionPlastic ABS · Thermal conductivity: base material: INEOS Styrolution Terluran GP-22 injection-molding ABS, typicalPlastic ABS · Thermal expansion: base material: INEOS Styrolution Terluran GP-22 injection-molding ABS, range
  9. 9
    Thermal Coefficient of Portland Cement ConcreteFederal Highway AdministrationConcrete · Thermal expansion: typical range for portland cement concrete (aggregate dependent)
  10. 10
    Best Practice Guidelines for Structural Fire Resistance Design of Concrete and Steel Buildings (TN 1681)National Institute of Standards and Technologyarchived copyConcrete · Specific heat: typical (NIST guidance for thermal analysis)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Plastic ABS is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Which is lighter, Concrete or Plastic ABS?

Plastic ABS is lighter: 1,100 kg/m³ against 2,320 kg/m³ for Concrete.

Which is stiffer, Concrete or Plastic ABS?

Concrete is stiffer: Young's modulus 25.1 GPa against 1.96 GPa for Plastic ABS, so the same part in Concrete deflects less under the same load.

Which is lighter for the same job, Concrete or Plastic ABS?

For the same stiffness or strength: Concrete is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate.

Part that must beConcretePlastic ABS
Stiff rod or tie (tension)lighter6.07x heavier
Stiff beam (bending)lighter1.7x heavier
Stiff panel or platelighter11% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Thermal

Which conducts heat better, Concrete or Plastic ABS?

Concrete conducts heat better: 0.9 W/m·K against 0.17 W/m·K for Plastic ABS.

Which expands less with temperature?

Concrete expands less: 10 µm/m·K against 95 µm/m·K for Plastic ABS.

Related comparisons