Materials / Compare

DMLS AlSi10Mg Aluminum vs. Steel AISI 1018

Compare DMLS AlSi10Mg Aluminum vs. Steel AISI 1018 strength, stiffness, weight and thermal properties.

DMLS AlSi10Mg Aluminum3D printed metal (DMLS)
Steel AISI 1018Wrought
MechanicalDMLS AlSi10Mg AluminumSteel AISI 1018
Yield strength270MPa1producer-stated372MPa238% stronger
Ultimate tensile strength450MPa1producer-stated441MPa2
Elongation at break10.2%1in 2 in15%247% more ductile
Young's modulus (stiffness)72GPa3base material200GPa4
Density2,670kg/m³5base material7,861kg/m³4
Strength to weight101kN·m/kg2.14x higher47.3kN·m/kg
Stiffness to weight27MN·m/kg6% higher25.4MN·m/kg
Poisson's ratiobase material0.334base material0.324
Shear modulus27.1GPa75.7GPa2.8x stiffer in shear
Bulk modulus70.6GPa185GPa2.62x higher
Speed of sound5,193m/s3% faster5,043m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumSteel AISI 1018
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumSteel AISI 1018
Strength against densityHigher and further left: stronger for its weight
ThermalDMLS AlSi10Mg AluminumSteel AISI 1018
Thermal conductivity110W/m·K1base material51.9W/m·K4
Thermal expansionmean 25-100 °C20µm/m·K1base material12µm/m·K61.67x less
100 mm part over a 50 °C swing100µm growth60µm growth1.67x less
Specific heatbase material963J/kg·K41.98x higherbase material486J/kg·K4
Heats up and cools (diffusivity)42.8mm²/s3.15x faster13.6mm²/s
Thermal shock resistance13,819W/m2.52x more resistant5,473W/m
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumSteel AISI 1018
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumStainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumSteel AISI 1018
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources6 documents: EOS GmbH, Niagara LaSalle, Renishaw, U.S. Department of Defense, Ovako
DMLS AlSi10Mg Aluminum
EOS Aluminium AlSi10Mg (powder 9011-0024), EOS M 290 | 30 µm process (AlSi10Mg_FlexM291 2.01), as manufactured, horizontal; machined (turned) specimens, ISO 6892-1 B10
Steel AISI 1018
AISI 1018 cold drawn bar (Niagara LaSalle, cold-finished bar producer)
  1. 1
    EOS Aluminium AlSi10Mg Material Data SheetEOS GmbHarchived copyDMLS AlSi10Mg Aluminum · Yield strength: typical, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Ultimate tensile strength: typical, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Elongation at break: typical at break, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Thermal conductivity: typical, as manufactured, horizontal (ISO 22007-2)DMLS AlSi10Mg Aluminum · Thermal expansion: mean 25-100 °C, ASTM E228
  2. 2
    1018 PropertiesNiagara LaSallearchived copySteel AISI 1018 · Yield strength: producer-stated, cold drawnSteel AISI 1018 · Ultimate tensile strength: producer-stated, cold drawnSteel AISI 1018 · Elongation at break: in 2 in (50.8 mm)
  3. 3
    RenAM 500 Series Aluminium AlSi10Mg Material Data SheetRenishawDMLS AlSi10Mg Aluminum · Young's modulus (stiffness): same material and process, different machine maker: Renishaw RenAM 500, 30 µm, as built, horizontal (XY)
  4. 4
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseSteel AISI 1018 · Young's modulus (stiffness): base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Density: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)DMLS AlSi10Mg Aluminum · Poisson's ratio: base material: cast Al-Si-Mg alloy 359.0 (Al-9Si-0.6Mg, closest MIL-HDBK-5J alloy to AlSi10Mg / EN AC-43000)Steel AISI 1018 · Poisson's ratio: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)Steel AISI 1018 · Thermal conductivity: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)DMLS AlSi10Mg Aluminum · Specific heat: base material: cast Al-Si-Mg alloy 359.0 (MIL-HDBK-5J), at 100 °CSteel AISI 1018 · Specific heat: base material: AISI 1025 plain carbon steel (MIL-HDBK-5J design value; ASTM A108 bar is the cold-finished carbon-steel bar spec that also covers 1018)
  5. 5
    EOS Aluminium AlSi10Mg Material Data Sheet, FlexLine, M 290 (2018)EOS GmbHarchived copyDMLS AlSi10Mg Aluminum · Density: typical part density (ISO 3369), EOS M 290, AlSi10Mg_030_FlexM291 (30 µm)
  6. 6
    S275JR Steel GradeOvakoSteel AISI 1018 · Thermal expansion: base material: unalloyed carbon steel, Ovako family table (S275JR, 'none alloyed structural steels', C <= 0.21%); mean 20-300 °C

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

DMLS AlSi10Mg Aluminum is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is DMLS AlSi10Mg Aluminum stronger than Steel AISI 1018?

Steel AISI 1018 is stronger: its yield strength is 372 MPa against 270 MPa for DMLS AlSi10Mg Aluminum (38%).

Which is lighter, DMLS AlSi10Mg Aluminum or Steel AISI 1018?

DMLS AlSi10Mg Aluminum is lighter: 2,670 kg/m³ against 7,861 kg/m³ for Steel AISI 1018.

Which is stiffer, DMLS AlSi10Mg Aluminum or Steel AISI 1018?

Steel AISI 1018 is stiffer: Young's modulus 200 GPa against 72 GPa for DMLS AlSi10Mg Aluminum, so the same part in Steel AISI 1018 deflects less under the same load.

Which is lighter for the same job, DMLS AlSi10Mg Aluminum or Steel AISI 1018?

For the same stiffness or strength: DMLS AlSi10Mg Aluminum is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beDMLS AlSi10Mg AluminumSteel AISI 1018
Stiff rod or tie (tension)lighter6% heavier
Stiff beam (bending)lighter1.77x heavier
Stiff panel or platelighter2.09x heavier
Strong rod or tielighter2.14x heavier
Strong beamlighter2.38x heavier
Strong panel or platelighter2.51x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, DMLS AlSi10Mg Aluminum or Steel AISI 1018?

Steel AISI 1018 stretches further before it breaks: 15% elongation at break against 10.2% for DMLS AlSi10Mg Aluminum.

Thermal

Which conducts heat better, DMLS AlSi10Mg Aluminum or Steel AISI 1018?

DMLS AlSi10Mg Aluminum conducts heat better: 110 W/m·K against 51.9 W/m·K for Steel AISI 1018.

Which expands less with temperature?

Steel AISI 1018 expands less: 12 µm/m·K against 20 µm/m·K for DMLS AlSi10Mg Aluminum.

Related comparisons