Materials / DMLS

DMLS AlSi10Mg Aluminum

DMLS AlSi10Mg Aluminum strength, stiffness, density and thermal properties, with their source.

A bracket in DMLS AlSi10Mg Aluminum, as-sintered finish.

Process3D printed metal (DMLS)
Mechanical
Yield strength270MPasourcetypical, as manufactured, horizontal
Ultimate tensile strength450MPasourcetypical, as manufactured, horizontal
Elongation at break10.2%sourcetypical at break, as manufactured, horizontal
Young's modulus (stiffness)72GPasourcesame material and process, different machine maker: Renishaw RenAM 500, 30 µm, as built, horizontal (XY)
Density2,670kg/m³sourcetypical part density (ISO 3369), EOS M 290, AlSi10Mg_030_FlexM291 (30 µm)
Strength to weight101kN·m/kg
Stiffness to weight27MN·m/kg
Poisson's ratio0.33sourcebase material: cast Al-Si-Mg alloy 359.0 (Al-9Si-0.6Mg, closest MIL-HDBK-5J alloy to AlSi10Mg / EN AC-43000)
Shear modulus27.1GPa
Bulk modulus70.6GPa
Speed of sound5,193m/s
Thermal
Thermal conductivity110W/m·Ksourcetypical, as manufactured, horizontal (ISO 22007-2)
Thermal expansion20µm/m·Ksourcemean 25-100 °C, ASTM E228
100 mm part over a 50 °C swing100µm growth
Specific heat963J/kg·Ksourcebase material: cast Al-Si-Mg alloy 359.0 (MIL-HDBK-5J), at 100 °C
Heats up and cools (diffusivity)42.8mm²/s
Thermal shock resistance13,819W/m
Values forEOS Aluminium AlSi10Mg (powder 9011-0024), EOS M 290 | 30 µm process (AlSi10Mg_FlexM291 2.01), as manufactured, horizontal; machined (turned) specimens, ISO 6892-1 B10

DMLS AlSi10Mg Aluminum is 3D printed: its properties depend on build direction and print settings; these are typical values.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelDMLS AlSi10Mg Aluminum
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickDMLS AlSi10Mg Aluminum
Strength against density

Compare DMLS AlSi10Mg Aluminum with