DMLS Ti-6Al-4V ELI Titanium vs. Plastic UHMWPE

Compare DMLS Ti-6Al-4V ELI Titanium vs. Plastic UHMWPE strength, stiffness, weight and thermal properties.

DMLS Ti-6Al-4V ELI Titanium3D printed metal (DMLS)
Plastic UHMWPEBulk polymer (molded or machined)
MechanicalDMLS Ti-6Al-4V ELI TitaniumPlastic UHMWPE
Yield strength1,100MPa155x stronger20MPa2
Ultimate tensile strength1,270MPa143MPa2
Elongation at break8.7%1465%253.4x more ductile
Young's modulus (stiffness)same maker and process110GPa3167x stiffer0.66GPa2
Density4,400kg/m³1930kg/m³24.73x lighter
Strength to weight250kN·m/kg11.6x higher21.5kN·m/kg
Stiffness to weight25MN·m/kg35.2x higher0.71MN·m/kg
Poisson's ratiowrought TIMETAL 6-40.3424not sourced
Shear modulus41GPanot sourced
Bulk modulus116GPanot sourced
Speed of sound5,000m/s5.94x faster842m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS Ti-6Al-4V ELI TitaniumPlastic UHMWPE
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS Ti-6Al-4V ELI TitaniumPlastic UHMWPE
Strength against densityHigher and further left: stronger for its weight
ThermalDMLS Ti-6Al-4V ELI TitaniumPlastic UHMWPE
Thermal conductivitybase material6.6W/m·K516.5x more heat through a fin0.4W/m·K6
Thermal expansionmean 25-100 °C9µm/m·K722.2x less200µm/m·K6
100 mm part over a 50 °C swing45µm growth22.2x less1,000µm growth
Specific heatbase material580J/kg·K5not sourced
Heats up and cools (diffusivity)2.59mm²/snot sourced
Thermal shock resistance4,825W/mnot sourced
Melting pointmelting range1,630–1,650°C4DSC 10 K/min130–138°C2
Max service temperaturenot sourced80°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS Ti-6Al-4V ELI TitaniumPlastic UHMWPE
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS Ti-6Al-4V ELI TitaniumPlastic UHMWPE
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources7 documents: EOS GmbH, Celanese, TIMET
DMLS Ti-6Al-4V ELI Titanium
EOS Titanium Ti64ELI (powder 9011-0040; ASTM F136/F3001, i.e. Grade 23) on EOS M400 SF, parameter set Ti64ELI_030_FlexM400_100, 30 µm, as built; ISO 6892-1 A14
Plastic UHMWPE
Celanese GUR 4120 (avg. molecular weight 4.7x10^6 g/mol), typical values on compression-molded specimens; CTE and thermal conductivity from Celanese's generic UHMWPE guide (grade not named)
  1. 1
    EOS Titanium Ti64ELI Material Data Sheet, M 290 and M 400EOS GmbHarchived copyDMLS Ti-6Al-4V ELI Titanium · Yield strength: typical, as built, average of horizontal + vertical (M400)DMLS Ti-6Al-4V ELI Titanium · Ultimate tensile strength: typical, as built, average of horizontal + vertical (M400)DMLS Ti-6Al-4V ELI Titanium · Elongation at break: typical at break, as built (M400)DMLS Ti-6Al-4V ELI Titanium · Density: typical part density (ISO 3369), M400
  2. 2
    GUR UHMW-PE Overview (GUR-015)CelanesePlastic UHMWPE · Yield strength: typical, tensile stress at yield ISO 527, 50 mm/minPlastic UHMWPE · Ultimate tensile strength: typical, tensile stress at break ISO 527, 50 mm/minPlastic UHMWPE · Elongation at break: typical, nominal elongation at break ISO 527Plastic UHMWPE · Young's modulus (stiffness): typical, tensile modulus ISO 527, 1 mm/minPlastic UHMWPE · Density: typicalPlastic UHMWPE · Melting point: DSC 10 K/minPlastic UHMWPE · Max service temperature: recommended max constant operating temperature
  3. 3
    EOS Titanium Ti64 Material Data Sheet, M 290 (2022)EOS GmbHarchived copyDMLS Ti-6Al-4V ELI Titanium · Young's modulus (stiffness): same maker and process, sibling grade: EOS Titanium Ti64 (Grade 5) on EOS M 290, as built, XY and Z, typical
  4. 4
    TIMETAL 6-4 PropertiesTIMETarchived copyDMLS Ti-6Al-4V ELI Titanium · Poisson's ratio: wrought TIMETAL 6-4 (TIMET measurement, mean of 10); composition-level, not DMLS-measuredDMLS Ti-6Al-4V ELI Titanium · Melting point: melting range, wrought TIMETAL 6-4 (composition-level)
  5. 5
    TIMETAL 6-4 Data SheetTIMETarchived copyDMLS Ti-6Al-4V ELI Titanium · Thermal conductivity: base material: wrought Ti-6Al-4V / 6-4 ELI (TIMET datasheet), 20 °CDMLS Ti-6Al-4V ELI Titanium · Specific heat: base material: wrought Ti-6Al-4V / 6-4 ELI (TIMET datasheet), 20 °C
  6. 6
    GUR UHMW-PE Polymer Guide (GUR-003)Celanesearchived copyPlastic UHMWPE · Thermal conductivity: typical, unfilled (narrative value, generic Celanese UHMWPE)Plastic UHMWPE · Thermal expansion: typical, 20 to 100 °C (generic Celanese UHMWPE)
  7. 7
    EOS Titanium Ti64 Grade 23 Material Data SheetEOS GmbHarchived copyDMLS Ti-6Al-4V ELI Titanium · Thermal expansion: mean 25-100 °C, ASTM E228; EOS Ti64 Grade 23 (=ELI) on EOS M 290 40 µm; condition not stated (sheet's mechanical data are heat treated)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

DMLS Ti-6Al-4V ELI Titanium is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is DMLS Ti-6Al-4V ELI Titanium stronger than Plastic UHMWPE?

DMLS Ti-6Al-4V ELI Titanium is stronger: its yield strength is 1,100 MPa against 20 MPa for Plastic UHMWPE (55x).

Which is lighter, DMLS Ti-6Al-4V ELI Titanium or Plastic UHMWPE?

Plastic UHMWPE is lighter: 930 kg/m³ against 4,400 kg/m³ for DMLS Ti-6Al-4V ELI Titanium.

Which is stiffer, DMLS Ti-6Al-4V ELI Titanium or Plastic UHMWPE?

DMLS Ti-6Al-4V ELI Titanium is stiffer: Young's modulus 110 GPa against 0.66 GPa for Plastic UHMWPE, so the same part in DMLS Ti-6Al-4V ELI Titanium deflects less under the same load.

Which is lighter for the same job, DMLS Ti-6Al-4V ELI Titanium or Plastic UHMWPE?

For the same stiffness or strength: DMLS Ti-6Al-4V ELI Titanium is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beDMLS Ti-6Al-4V ELI TitaniumPlastic UHMWPE
Stiff rod or tie (tension)lighter35.2x heavier
Stiff beam (bending)lighter2.73x heavier
Stiff panel or platelighter16% heavier
Strong rod or tielighter11.6x heavier
Strong beamlighter3.06x heavier
Strong panel or platelighter1.57x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, DMLS Ti-6Al-4V ELI Titanium or Plastic UHMWPE?

Plastic UHMWPE stretches further before it breaks: 465% elongation at break against 8.7% for DMLS Ti-6Al-4V ELI Titanium.

Thermal

Which conducts heat better, DMLS Ti-6Al-4V ELI Titanium or Plastic UHMWPE?

DMLS Ti-6Al-4V ELI Titanium conducts heat better: 6.6 W/m·K against 0.4 W/m·K for Plastic UHMWPE.

Which expands less with temperature?

DMLS Ti-6Al-4V ELI Titanium expands less: 9 µm/m·K against 200 µm/m·K for Plastic UHMWPE.