Materials / Compare

FDM ASA vs. Magnesium AZ31B-H24

Compare FDM ASA vs. Magnesium AZ31B-H24 strength, stiffness, weight and thermal properties.

FDM ASA3D printed (FDM)
Magnesium AZ31B-H24Wrought
MechanicalFDM ASAMagnesium AZ31B-H24
Yield strengthnot given (tensile used)220MPa1
Ultimate tensile strength37MPa2290MPa17.84x stronger
Flexural strength65MPa2not sourced
Elongation at break9.2%213%141% more ductile
Young's modulus (stiffness)2.45GPa244.8GPa318.3x stiffer
Density1,050kg/m³21.68x lighter1,769kg/m³3
Strength to weight35.2kN·m/kg124kN·m/kg3.53x higher
Stiffness to weight2.33MN·m/kg25.3MN·m/kg10.9x higher
Poisson's rationot sourced0.353
Shear modulusnot sourced16.6GPa
Bulk modulusnot sourced49.8GPa
Speed of sound1,528m/s5,032m/s3.29x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASAMagnesium AZ31B-H24
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASAMagnesium AZ31B-H24
Strength against densityHigher and further left: stronger for its weight
ThermalFDM ASAMagnesium AZ31B-H24
Thermal conductivitybase material0.17W/m·K476.9W/m·K1452x more heat through a fin
Thermal expansionbase material80–110µm/m·K426.8µm/m·K1
100 mm part over a 50 °C swing475µm growth134µm growth3.54x less
Specific heatnot sourced1,040J/kg·K1
Heats up and cools (diffusivity)not sourced41.8mm²/s
Thermal shock resistancenot sourced9,159W/m
Max service temperatureHDT 1.8 MPa92°C2149°C3
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASAMagnesium AZ31B-H24
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASAMagnesium AZ31B-H24
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Magnesium Elektron, Bambu Lab, U.S. Department of Defense, INEOS Styrolution
FDM ASA
Bambu Lab ASA, TDS V3.0, printed specimens X-Y; nozzle 260 °C, bed 80 °C, 200 mm/s, 100% infill; annealed and dried 80 °C for 12 h before testing.
Magnesium AZ31B-H24
AZ31B-H24 sheet 0.016-0.062 in., MIL-HDBK-5J Table 4.2.1.0(b) (AMS 4377); strengths are S-basis MINIMUMS
  1. 1
    Elektron AZ31B Sheet, Plate & Coil (Datasheet 482)Magnesium Elektronarchived copyMagnesium AZ31B-H24 · Yield strength: typical, H24, 0.5-6 mm, 0.2 % proof stressMagnesium AZ31B-H24 · Ultimate tensile strength: typical, H24, 0.5-6 mmMagnesium AZ31B-H24 · Elongation at break: typical, H24, 0.5-6 mm, gauge 5.65√AMagnesium AZ31B-H24 · Thermal conductivity: typical (temper/temperature not stated)Magnesium AZ31B-H24 · Thermal expansion: typical (temperature range not stated)Magnesium AZ31B-H24 · Specific heat: typical
  2. 2
    Bambu ASA Technical Data Sheet, V3.0Bambu LabFDM ASA · Ultimate tensile strength: typicalFDM ASA · Flexural strength: typicalFDM ASA · Elongation at break: typicalFDM ASA · Young's modulus (stiffness): typicalFDM ASA · Density: typicalFDM ASA · Max service temperature: HDT 1.8 MPa
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseMagnesium AZ31B-H24 · Young's modulus (stiffness): typical (handbook physical constant)Magnesium AZ31B-H24 · Density: nominalMagnesium AZ31B-H24 · Poisson's ratio: typical (handbook physical constant)Magnesium AZ31B-H24 · Max service temperature: stated application limit
  4. 4
    Luran S 777K (ASA) Product Data SheetINEOS StyrolutionFDM ASA · Thermal conductivity: base material: INEOS Styrolution Luran S 777K injection-molding ASA, typicalFDM ASA · Thermal expansion: base material: INEOS Styrolution Luran S 777K injection-molding ASA, range

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

FDM ASA is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is FDM ASA stronger than Magnesium AZ31B-H24?

Magnesium AZ31B-H24 is stronger: its yield strength is 220 MPa against tensile strength 37 MPa for FDM ASA (5.95x).

Which is lighter, FDM ASA or Magnesium AZ31B-H24?

FDM ASA is lighter: 1,050 kg/m³ against 1,769 kg/m³ for Magnesium AZ31B-H24.

Which is stiffer, FDM ASA or Magnesium AZ31B-H24?

Magnesium AZ31B-H24 is stiffer: Young's modulus 44.8 GPa against 2.45 GPa for FDM ASA, so the same part in Magnesium AZ31B-H24 deflects less under the same load.

Which is lighter for the same job, FDM ASA or Magnesium AZ31B-H24?

For the same stiffness or strength: Magnesium AZ31B-H24 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beFDM ASAMagnesium AZ31B-H24
Stiff rod or tie (tension)10.9x heavierlighter
Stiff beam (bending)2.54x heavierlighter
Stiff panel or plate1.56x heavierlighter
Strong rod or tie3.53x heavierlighter
Strong beam1.95x heavierlighter
Strong panel or plate45% heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, FDM ASA or Magnesium AZ31B-H24?

Magnesium AZ31B-H24 stretches further before it breaks: 13% elongation at break against 9.2% for FDM ASA.

Thermal

Which conducts heat better, FDM ASA or Magnesium AZ31B-H24?

Magnesium AZ31B-H24 conducts heat better: 76.9 W/m·K against 0.17 W/m·K for FDM ASA.

Which expands less with temperature?

Magnesium AZ31B-H24 expands less: 26.8 µm/m·K against 95 µm/m·K for FDM ASA.

Related comparisons