MechanicalFDM ASASLA Resin Elastic 50A
Yield strengthnot given (tensile used)not given (tensile used)
Ultimate tensile strength37MPa110.9x stronger3.4MPa2
Flexural strength65MPa1not sourced
Elongation at break9.2%1160%217.4x more ductile
Young's modulus (stiffness)2.45GPa1not sourced
Density1,050kg/m³11,010kg/m³2
Strength to weight35.2kN·m/kg10.5x higher3.37kN·m/kg
Stiffness to weight2.33MN·m/kgnot sourced
Poisson's rationot sourcednot sourced
Shear modulusnot sourcednot sourced
Bulk modulusnot sourcednot sourced
Speed of sound1,528m/snot sourced
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASA
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASASLA Resin Elastic 50A
Strength against densityHigher and further left: stronger for its weight
ThermalFDM ASASLA Resin Elastic 50A
Thermal conductivitybase material0.17W/m·K3not sourced
Thermal expansionbase material80–110µm/m·K3not sourced
100 mm part over a 50 °C swing475µm growthnot sourced
Specific heatnot sourcednot sourced
Heats up and cools (diffusivity)not sourcednot sourced
Thermal shock resistancenot sourcednot sourced
Glass transitionnot sourcedDMA-34.5°C2
Max service temperatureHDT 1.8 MPa92°C1not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASA
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASA
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources3 documents: Bambu Lab, Formlabs, INEOS Styrolution
FDM ASA
Bambu Lab ASA, TDS V3.0, printed specimens X-Y; nozzle 260 °C, bed 80 °C, 200 mm/s, 100% infill; annealed and dried 80 °C for 12 h before testing.
SLA Resin Elastic 50A
Formlabs Elastic 50A Resin V2 (FLELCL02), TDS Rev. 01 24.01.2024; parts printed on Form 3, 100 µm, Elastic 50A V2 settings and post-processing; tensile on Die C specimens cut from printed sheets after 3+ h at 23 °C.
  1. 1
    Bambu ASA Technical Data Sheet, V3.0Bambu LabFDM ASA · Ultimate tensile strength: typicalFDM ASA · Flexural strength: typicalFDM ASA · Elongation at break: typicalFDM ASA · Young's modulus (stiffness): typicalFDM ASA · Density: typicalFDM ASA · Max service temperature: HDT 1.8 MPa
  2. 2
    Elastic 50A Resin V2 Technical Data Sheet (2024)Formlabsarchived copySLA Resin Elastic 50A · Ultimate tensile strength: typicalSLA Resin Elastic 50A · Elongation at break: typicalSLA Resin Elastic 50A · Density: typicalSLA Resin Elastic 50A · Glass transition: DMA
  3. 3
    Luran S 777K (ASA) Product Data SheetINEOS StyrolutionFDM ASA · Thermal conductivity: base material: INEOS Styrolution Luran S 777K injection-molding ASA, typicalFDM ASA · Thermal expansion: base material: INEOS Styrolution Luran S 777K injection-molding ASA, range

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

FDM ASA and SLA Resin Elastic 50A are 3D printed: their properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is FDM ASA stronger than SLA Resin Elastic 50A?

FDM ASA is stronger: its tensile strength is 37 MPa against 3.4 MPa for SLA Resin Elastic 50A (10.9x).

Which is lighter, FDM ASA or SLA Resin Elastic 50A?

SLA Resin Elastic 50A is lighter: 1,010 kg/m³ against 1,050 kg/m³ for FDM ASA.

Which is lighter for the same job, FDM ASA or SLA Resin Elastic 50A?

For the same stiffness or strength: FDM ASA is lighter for a strong rod or tie, strong beam, strong panel or plate.

Part that must beFDM ASASLA Resin Elastic 50A
Strong rod or tielighter10.5x heavier
Strong beamlighter4.72x heavier
Strong panel or platelighter3.17x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, FDM ASA or SLA Resin Elastic 50A?

SLA Resin Elastic 50A stretches further before it breaks: 160% elongation at break against 9.2% for FDM ASA.

Related comparisons