FDM Polycarbonate3D printed (FDM)
Stainless Steel 303Wrought
MechanicalFDM PolycarbonateStainless Steel 303
Yield strength53.3MPa1Outokumpu typical275MPa25.16x stronger
Ultimate tensile strength53.3MPa1Outokumpu typical585MPa211x stronger
Flexural strength89.4MPa1not sourced
Elongation at break9.2%1Outokumpu typical35%23.8x more ductile
Young's modulus (stiffness)2.39GPa1at RT200GPa283.5x stiffer
Densityrange1,180–1,200kg/m³1at RT7,900kg/m³2
Strength to weight44.8kN·m/kg29% higher34.8kN·m/kg
Stiffness to weight2.01MN·m/kg25.3MN·m/kg12.6x higher
Poisson's ratiobase material0.383design value0.34
Shear modulus0.867GPa76.9GPa88.7x stiffer in shear
Bulk modulus3.33GPa167GPa50.1x higher
Speed of sound1,418m/s5,032m/s3.55x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM PolycarbonateStainless Steel 303
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM PolycarbonateStainless Steel 303
Strength against densityHigher and further left: stronger for its weight
ThermalFDM PolycarbonateStainless Steel 303
Thermal conductivitybase material0.2W/m·K5at RT15W/m·K275x more heat through a fin
Thermal expansionbase material65µm/m·K5mean16µm/m·K24.06x less
100 mm part over a 50 °C swing325µm growth80µm growth4.06x less
Specific heatnot sourcedat RT500J/kg·K2
Heats up and cools (diffusivity)not sourced3.8mm²/s
Thermal shock resistance42.5W/m902W/m21.2x more resistant
Glass transition108°C1not sourced
Max service temperatureHDT 0.455 MPa105°C1continuous871°C6
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM PolycarbonateStainless Steel 303
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM PolycarbonateStainless Steel 303
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources6 documents: UltiMaker, Outokumpu, Covestro, Steel Construction Institute, Carpenter Technology
FDM Polycarbonate
Ultimaker PC, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS (file v5.00), April 20, 2022.
Stainless Steel 303
1.4305 / UNS S30300, Outokumpu typical values (hot rolled, solution annealed) from 'Steel Grades, Properties and Global Standards'; max service from Carpenter CarTech 303 datasheet
  1. 1
    Ultimaker PC Technical Data Sheet, v5.00UltiMakerarchived copyFDM Polycarbonate · Yield strength: typicalFDM Polycarbonate · Ultimate tensile strength: typical, peak stress (= stress at yield)FDM Polycarbonate · Flexural strength: typicalFDM Polycarbonate · Elongation at break: typicalFDM Polycarbonate · Young's modulus (stiffness): typicalFDM Polycarbonate · Density: rangeFDM Polycarbonate · Glass transition: typicalFDM Polycarbonate · Max service temperature: HDT 0.455 MPa (printed specimens)
  2. 2
    Steel Grades, Properties and Global StandardsOutokumpuarchived copyStainless Steel 303 · Yield strength: Outokumpu typical (product P = hot rolled plate, transverse)Stainless Steel 303 · Ultimate tensile strength: Outokumpu typicalStainless Steel 303 · Elongation at break: Outokumpu typical, A5Stainless Steel 303 · Young's modulus (stiffness): at RT (Table 12)Stainless Steel 303 · Density: at RTStainless Steel 303 · Thermal conductivity: at RTStainless Steel 303 · Thermal expansion: mean, 20–100 °CStainless Steel 303 · Specific heat: at RT
  3. 3
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroarchived copyFDM Polycarbonate · Poisson's ratio: base material: polycarbonate family typical (Covestro Part and Mold Design guide, Table 3-1)
  4. 4
    Design Manual for Structural Stainless Steel, 4th Edition (P413)Steel Construction Institutearchived copyStainless Steel 303 · Poisson's ratio: design value (structural stainless steels)
  5. 5
    Makrolon 2405 Technical Data SheetCovestroFDM Polycarbonate · Thermal conductivity: base material: Covestro Makrolon 2405 injection-molding PC, typical, through-plane, 23 °CFDM Polycarbonate · Thermal expansion: base material: Covestro Makrolon 2405 injection-molding PC, typical, 23-55 °C, parallel
  6. 6
    Carpenter Stainless Type 303 Data SheetCarpenter Technologyarchived copyStainless Steel 303 · Max service temperature: continuous, scaling limit

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

FDM Polycarbonate is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is FDM Polycarbonate stronger than Stainless Steel 303?

Stainless Steel 303 is stronger: its yield strength is 275 MPa against 53.3 MPa for FDM Polycarbonate (5.16x).

Which is lighter, FDM Polycarbonate or Stainless Steel 303?

FDM Polycarbonate is lighter: 1,190 kg/m³ against 7,900 kg/m³ for Stainless Steel 303.

Which is stiffer, FDM Polycarbonate or Stainless Steel 303?

Stainless Steel 303 is stiffer: Young's modulus 200 GPa against 2.39 GPa for FDM Polycarbonate, so the same part in Stainless Steel 303 deflects less under the same load.

Which is lighter for the same job, FDM Polycarbonate or Stainless Steel 303?

For the same stiffness or strength: FDM Polycarbonate is lighter for a stiff panel or plate, strong rod or tie, strong beam, strong panel or plate; Stainless Steel 303 is lighter for a stiff rod or tie (tension), stiff beam (bending).

Part that must beFDM PolycarbonateStainless Steel 303
Stiff rod or tie (tension)12.6x heavierlighter
Stiff beam (bending)38% heavierlighter
Stiff panel or platelighter1.52x heavier
Strong rod or tielighter29% heavier
Strong beamlighter2.22x heavier
Strong panel or platelighter2.92x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, FDM Polycarbonate or Stainless Steel 303?

Stainless Steel 303 stretches further before it breaks: 35% elongation at break against 9.2% for FDM Polycarbonate.

Thermal

Which conducts heat better, FDM Polycarbonate or Stainless Steel 303?

Stainless Steel 303 conducts heat better: 15 W/m·K against 0.2 W/m·K for FDM Polycarbonate.

Which expands less with temperature?

Stainless Steel 303 expands less: 16 µm/m·K against 65 µm/m·K for FDM Polycarbonate.

Related comparisons