Materials / FDM

FDM Polycarbonate

FDM Polycarbonate (PC) strength, stiffness, density and thermal properties, with their source.

A bracket in FDM Polycarbonate, 3D-printed (layer lines) finish.

Process3D printed (FDM)
Mechanical
Yield strength53.3MPasourcetypical
Ultimate tensile strength53.3MPasourcetypical, peak stress (= stress at yield)
Flexural strength89.4MPasourcetypical
Elongation at break9.2%sourcetypical
Young's modulus (stiffness)2.39GPasourcetypical
Density1,180–1,200kg/m³sourcerange
Strength to weight44.8kN·m/kg
Stiffness to weight2.01MN·m/kg
Poisson's ratio0.38sourcebase material: polycarbonate family typical (Covestro Part and Mold Design guide, Table 3-1)
Shear modulus0.867GPa
Bulk modulus3.33GPa
Speed of sound1,418m/s
Thermal
Thermal conductivity0.2W/m·Ksourcebase material: Covestro Makrolon 2405 injection-molding PC, typical, through-plane, 23 °C
Thermal expansion65µm/m·Ksourcebase material: Covestro Makrolon 2405 injection-molding PC, typical, 23-55 °C, parallel
100 mm part over a 50 °C swing325µm growth
Specific heatnot sourced
Heats up and cools (diffusivity)not sourced
Thermal shock resistance42.5W/m
Glass transition108°Csourcetypical
Max service temperature105°CsourceHDT 0.455 MPa (printed specimens)
Values forUltimaker PC, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS (file v5.00), April 20, 2022.

FDM Polycarbonate is 3D printed: its properties depend on build direction and print settings; these are typical values.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelFDM Polycarbonate
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickFDM Polycarbonate
Strength against density

Compare FDM Polycarbonate with