Materials / Compare

Magnesium AZ31B-H24 vs. Plastic Nylon PA66

Compare Magnesium AZ31B-H24 vs. Plastic Nylon PA66 strength, stiffness, weight and thermal properties.

Magnesium AZ31B-H24Wrought
Plastic Nylon PA66Bulk polymer (molded or machined)
MechanicalMagnesium AZ31B-H24Plastic Nylon PA66
Yield strength220MPa12.59x stronger85MPa2
Ultimate tensile strength290MPa1not stated (yield given)
Elongation at break13%130%22.31x more ductile
Young's modulus (stiffness)44.8GPa314.9x stiffer3GPa2
Density1,769kg/m³31,130kg/m³21.57x lighter
Strength to weight124kN·m/kg1.65x higher75.2kN·m/kg
Stiffness to weight25.3MN·m/kg9.54x higher2.65MN·m/kg
Poisson's ratio0.353base material0.44
Shear modulus16.6GPa15.5x stiffer in shear1.07GPa
Bulk modulus49.8GPa9.96x higher5GPa
Speed of sound5,032m/s3.09x faster1,629m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Plastic Nylon PA66
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Plastic Nylon PA66
Strength against densityHigher and further left: stronger for its weight
ThermalMagnesium AZ31B-H24Plastic Nylon PA66
Thermal conductivity76.9W/m·K1233x more heat through a fin0.33W/m·K2
Thermal expansion26.8µm/m·K13.66x lesslongitudinal98µm/m·K2
100 mm part over a 50 °C swing134µm growth3.66x less490µm growth
Specific heat1,040J/kg·K11,700J/kg·K21.63x higher
Heats up and cools (diffusivity)41.8mm²/s243x faster0.172mm²/s
Thermal shock resistance9,159W/m160x more resistant57.2W/m
Melting pointnot sourcedDSC260°C2
Max service temperature149°C348 °C hotter101°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Plastic Nylon PA66
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Plastic Nylon PA66
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Magnesium Elektron, BASF, U.S. Department of Defense, Covestro
Magnesium AZ31B-H24
AZ31B-H24 sheet 0.016-0.062 in., MIL-HDBK-5J Table 4.2.1.0(b) (AMS 4377); strengths are S-basis MINIMUMS
Plastic Nylon PA66
BASF Ultramid A3K (PA66, unreinforced injection-moulding grade), Product Information 02/2026, dry values (ISO methods)
  1. 1
    Elektron AZ31B Sheet, Plate & Coil (Datasheet 482)Magnesium Elektronarchived copyMagnesium AZ31B-H24 · Yield strength: typical, H24, 0.5-6 mm, 0.2 % proof stressMagnesium AZ31B-H24 · Ultimate tensile strength: typical, H24, 0.5-6 mmMagnesium AZ31B-H24 · Elongation at break: typical, H24, 0.5-6 mm, gauge 5.65√AMagnesium AZ31B-H24 · Thermal conductivity: typical (temper/temperature not stated)Magnesium AZ31B-H24 · Thermal expansion: typical (temperature range not stated)Magnesium AZ31B-H24 · Specific heat: typical
  2. 2
    Ultramid A3K Product InformationBASFPlastic Nylon PA66 · Yield strength: typical, dryPlastic Nylon PA66 · Elongation at break: nominal strain at break, dryPlastic Nylon PA66 · Young's modulus (stiffness): typical, dryPlastic Nylon PA66 · Density: typicalPlastic Nylon PA66 · Thermal conductivity: typicalPlastic Nylon PA66 · Thermal expansion: longitudinal, 23-55 °CPlastic Nylon PA66 · Specific heat: typicalPlastic Nylon PA66 · Melting point: DSCPlastic Nylon PA66 · Max service temperature: IEC 60216 temperature index, 20000 h
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseMagnesium AZ31B-H24 · Young's modulus (stiffness): typical (handbook physical constant)Magnesium AZ31B-H24 · Density: nominalMagnesium AZ31B-H24 · Poisson's ratio: typical (handbook physical constant)Magnesium AZ31B-H24 · Max service temperature: stated application limit
  4. 4
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroPlastic Nylon PA66 · Poisson's ratio: base material: unfilled polyamide (PA), conditioned, maker design-guide family value (Covestro Table 3-1)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Magnesium AZ31B-H24 stronger than Plastic Nylon PA66?

Magnesium AZ31B-H24 is stronger: its yield strength is 220 MPa against 85 MPa for Plastic Nylon PA66 (2.59x).

Which is lighter, Magnesium AZ31B-H24 or Plastic Nylon PA66?

Plastic Nylon PA66 is lighter: 1,130 kg/m³ against 1,769 kg/m³ for Magnesium AZ31B-H24.

Which is stiffer, Magnesium AZ31B-H24 or Plastic Nylon PA66?

Magnesium AZ31B-H24 is stiffer: Young's modulus 44.8 GPa against 3 GPa for Plastic Nylon PA66, so the same part in Magnesium AZ31B-H24 deflects less under the same load.

Which is lighter for the same job, Magnesium AZ31B-H24 or Plastic Nylon PA66?

For the same stiffness or strength: Magnesium AZ31B-H24 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beMagnesium AZ31B-H24Plastic Nylon PA66
Stiff rod or tie (tension)lighter9.54x heavier
Stiff beam (bending)lighter2.47x heavier
Stiff panel or platelighter1.57x heavier
Strong rod or tielighter1.65x heavier
Strong beamlighter20% heavier
Strong panel or platelighter3% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Magnesium AZ31B-H24 or Plastic Nylon PA66?

Plastic Nylon PA66 stretches further before it breaks: 30% elongation at break against 13% for Magnesium AZ31B-H24.

Thermal

Which handles higher temperatures, Magnesium AZ31B-H24 or Plastic Nylon PA66?

Magnesium AZ31B-H24 does: 149 °C against 101 °C for Plastic Nylon PA66.

Which conducts heat better, Magnesium AZ31B-H24 or Plastic Nylon PA66?

Magnesium AZ31B-H24 conducts heat better: 76.9 W/m·K against 0.33 W/m·K for Plastic Nylon PA66.

Which expands less with temperature?

Magnesium AZ31B-H24 expands less: 26.8 µm/m·K against 98 µm/m·K for Plastic Nylon PA66.