Materials / Compare

Plastic ABS (bulk/injection) vs. SLA Resin Elastic 50A

Compare Plastic ABS (bulk/injection) vs. SLA Resin Elastic 50A strength, stiffness, weight and thermal properties.

Plastic ABS (bulk/injection)Bulk polymer (molded or machined)
SLA Resin Elastic 50A3D printed (SLA resin)
MechanicalPlastic ABS (bulk/injection)SLA Resin Elastic 50A
Yield strength45MPa1not given (tensile used)
Ultimate tensile strengthnot stated (yield given)3.4MPa2
Flexural strength65MPa1not sourced
Elongation at break10%1160%216x more ductile
Young's modulus (stiffness)2.3GPa1not sourced
Density1,040kg/m³11,010kg/m³2
Strength to weight43.3kN·m/kg12.9x higher3.37kN·m/kg
Stiffness to weight2.21MN·m/kgnot sourced
Poisson's ratio0.393not sourced
Shear modulus0.827GPanot sourced
Bulk modulus3.48GPanot sourced
Speed of sound1,487m/snot sourced
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic ABS (bulk/injection)
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic ABS (bulk/injection)SLA Resin Elastic 50A
Strength against densityHigher and further left: stronger for its weight
ThermalPlastic ABS (bulk/injection)SLA Resin Elastic 50A
Thermal conductivity0.17W/m·K1not sourced
Thermal expansionrange80–110µm/m·K1not sourced
100 mm part over a 50 °C swing475µm growthnot sourced
Specific heatnot sourcednot sourced
Heats up and cools (diffusivity)not sourcednot sourced
Thermal shock resistance21.4W/mnot sourced
Glass transitionnot sourcedDMA-34.5°C2
Max service temperatureHDT 1.8 MPa94°C1not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic ABS (bulk/injection)
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic ABS (bulk/injection)
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources3 documents: INEOS Styrolution, Formlabs, Covestro
Plastic ABS (bulk/injection)
INEOS Styrolution Terluran GP-22 general-purpose injection-molding ABS, ISO typical values (TDS revision 08/01/2022)
SLA Resin Elastic 50A
Formlabs Elastic 50A Resin V2 (FLELCL02), TDS Rev. 01 24.01.2024; parts printed on Form 3, 100 µm, Elastic 50A V2 settings and post-processing; tensile on Die C specimens cut from printed sheets after 3+ h at 23 °C.
  1. 1
    Terluran GP-22 (ABS) Product Data SheetINEOS StyrolutionPlastic ABS (bulk/injection) · Yield strength: typical, tensile stress at yield 23 °CPlastic ABS (bulk/injection) · Flexural strength: typical, 23 °CPlastic ABS (bulk/injection) · Elongation at break: nominal strain at break, 23 °CPlastic ABS (bulk/injection) · Young's modulus (stiffness): typicalPlastic ABS (bulk/injection) · Density: typicalPlastic ABS (bulk/injection) · Thermal conductivity: typicalPlastic ABS (bulk/injection) · Thermal expansion: rangePlastic ABS (bulk/injection) · Max service temperature: HDT 1.8 MPa (annealed 4 h/80 °C)
  2. 2
    Elastic 50A Resin V2 Technical Data Sheet (2024)Formlabsarchived copySLA Resin Elastic 50A · Ultimate tensile strength: typicalSLA Resin Elastic 50A · Elongation at break: typicalSLA Resin Elastic 50A · Density: typicalSLA Resin Elastic 50A · Glass transition: DMA
  3. 3
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroarchived copyPlastic ABS (bulk/injection) · Poisson's ratio: typical, ABS family (Covestro Part and Mold Design guide, Table 3-1)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

SLA Resin Elastic 50A is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Plastic ABS (bulk/injection) stronger than SLA Resin Elastic 50A?

Plastic ABS (bulk/injection) is stronger: its yield strength is 45 MPa against tensile strength 3.4 MPa for SLA Resin Elastic 50A (13.2x).

Which is lighter, Plastic ABS (bulk/injection) or SLA Resin Elastic 50A?

SLA Resin Elastic 50A is lighter: 1,010 kg/m³ against 1,040 kg/m³ for Plastic ABS (bulk/injection).

Which is lighter for the same job, Plastic ABS (bulk/injection) or SLA Resin Elastic 50A?

For the same stiffness or strength: Plastic ABS (bulk/injection) is lighter for a strong rod or tie, strong beam, strong panel or plate.

Part that must bePlastic ABS (bulk/injection)SLA Resin Elastic 50A
Strong rod or tielighter12.9x heavier
Strong beamlighter5.43x heavier
Strong panel or platelighter3.53x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Plastic ABS (bulk/injection) or SLA Resin Elastic 50A?

SLA Resin Elastic 50A stretches further before it breaks: 160% elongation at break against 10% for Plastic ABS (bulk/injection).

Related comparisons