MechanicalPlastic Nylon PA66Stainless Steel 17-4PH
Yield strength85MPa11,275MPa215x stronger
Ultimate tensile strengthnot stated (yield given)1,379MPa2
Elongation at break30%13.33x more ductile9%2
Young's modulus (stiffness)3GPa1H 900197GPa265.7x stiffer
Density1,130kg/m³16.9x lighterH 9007,800kg/m³2
Strength to weight75.2kN·m/kg163kN·m/kg2.17x higher
Stiffness to weight2.65MN·m/kg25.3MN·m/kg9.51x higher
Poisson's ratiobase material0.43H 9000.2722
Shear modulus1.07GPa77.4GPa72.3x stiffer in shear
Bulk modulus5GPa144GPa28.8x higher
Speed of sound1,629m/s5,026m/s3.08x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic Nylon PA66Stainless Steel 17-4PH
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic Nylon PA66Stainless Steel 17-4PH
Strength against densityHigher and further left: stronger for its weight
ThermalPlastic Nylon PA66Stainless Steel 17-4PH
Thermal conductivity0.33W/m·K1at 149 °C17.9W/m·K254.2x more heat through a fin
Thermal expansionlongitudinal98µm/m·K1mean10.8µm/m·K29.07x less
100 mm part over a 50 °C swing490µm growth54µm growth9.07x less
Specific heat1,700J/kg·K13.7x highermean460J/kg·K2
Heats up and cools (diffusivity)0.172mm²/s4.99mm²/s29x faster
Thermal shock resistance57.2W/m7,809W/m136x more resistant
Melting pointDSC260°C1not sourced
Max service temperature101°C1316°C2215 °C hotter
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic Nylon PA66Stainless Steel 17-4PH
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic Nylon PA66Stainless Steel 17-4PH
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources3 documents: BASF, Cleveland-Cliffs, Covestro
Plastic Nylon PA66
BASF Ultramid A3K (PA66, unreinforced injection-moulding grade), Product Information 02/2026, dry values (ISO methods)
Stainless Steel 17-4PH
Cleveland-Cliffs 17-4 PH, Condition H 900, sheet/strip, transverse (Product Data Bulletin, May 2021)
  1. 1
    Ultramid A3K Product InformationBASFPlastic Nylon PA66 · Yield strength: typical, dryPlastic Nylon PA66 · Elongation at break: nominal strain at break, dryPlastic Nylon PA66 · Young's modulus (stiffness): typical, dryPlastic Nylon PA66 · Density: typicalPlastic Nylon PA66 · Thermal conductivity: typicalPlastic Nylon PA66 · Thermal expansion: longitudinal, 23-55 °CPlastic Nylon PA66 · Specific heat: typicalPlastic Nylon PA66 · Melting point: DSCPlastic Nylon PA66 · Max service temperature: IEC 60216 temperature index, 20000 h
  2. 2
    17-4 PH Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsStainless Steel 17-4PH · Yield strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Ultimate tensile strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Elongation at break: typical, transverse, in 2 in. (50.8 mm)Stainless Steel 17-4PH · Young's modulus (stiffness): H 900Stainless Steel 17-4PH · Density: H 900Stainless Steel 17-4PH · Poisson's ratio: H 900 (column)Stainless Steel 17-4PH · Thermal conductivity: at 149 °C (300 °F), H 900Stainless Steel 17-4PH · Thermal expansion: mean, 21–93 °C (70–200 °F), H 900Stainless Steel 17-4PH · Specific heat: mean, 0–100 °C, H 900Stainless Steel 17-4PH · Max service temperature: strength-retention limit (not oxidation)
  3. 3
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroPlastic Nylon PA66 · Poisson's ratio: base material: unfilled polyamide (PA), conditioned, maker design-guide family value (Covestro Table 3-1)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Plastic Nylon PA66 stronger than Stainless Steel 17-4PH?

Stainless Steel 17-4PH is stronger: its yield strength is 1,275 MPa against 85 MPa for Plastic Nylon PA66 (15x).

Which is lighter, Plastic Nylon PA66 or Stainless Steel 17-4PH?

Plastic Nylon PA66 is lighter: 1,130 kg/m³ against 7,800 kg/m³ for Stainless Steel 17-4PH.

Which is stiffer, Plastic Nylon PA66 or Stainless Steel 17-4PH?

Stainless Steel 17-4PH is stiffer: Young's modulus 197 GPa against 3 GPa for Plastic Nylon PA66, so the same part in Stainless Steel 17-4PH deflects less under the same load.

Which is lighter for the same job, Plastic Nylon PA66 or Stainless Steel 17-4PH?

For the same stiffness or strength: Plastic Nylon PA66 is lighter for a stiff panel or plate, strong beam, strong panel or plate; Stainless Steel 17-4PH is lighter for a stiff rod or tie (tension), stiff beam (bending), strong rod or tie.

Part that must bePlastic Nylon PA66Stainless Steel 17-4PH
Stiff rod or tie (tension)9.51x heavierlighter
Stiff beam (bending)17% heavierlighter
Stiff panel or platelighter1.71x heavier
Strong rod or tie2.17x heavierlighter
Strong beamlighter13% heavier
Strong panel or platelighter1.78x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Plastic Nylon PA66 or Stainless Steel 17-4PH?

Plastic Nylon PA66 stretches further before it breaks: 30% elongation at break against 9% for Stainless Steel 17-4PH.

Thermal

Which handles higher temperatures, Plastic Nylon PA66 or Stainless Steel 17-4PH?

Stainless Steel 17-4PH does: 316 °C against 101 °C for Plastic Nylon PA66.

Which conducts heat better, Plastic Nylon PA66 or Stainless Steel 17-4PH?

Stainless Steel 17-4PH conducts heat better: 17.9 W/m·K against 0.33 W/m·K for Plastic Nylon PA66.

Which expands less with temperature?

Stainless Steel 17-4PH expands less: 10.8 µm/m·K against 98 µm/m·K for Plastic Nylon PA66.