Materials / Compare

Plywood vs. Zinc Zamak 3

Compare Plywood vs. Zinc Zamak 3 strength, stiffness, weight and thermal properties.

PlywoodNatural
Zinc Zamak 3Cast
MechanicalPlywoodZinc Zamak 3
Yield strengthnot given (tensile used)221MPa1
Ultimate tensile strengthmodulus of rupture41.4MPa2283MPa1
Flexural strengthstatic bending MOR41.4MPa2not sourced
Elongation at breaknot sourced10%1
Young's modulus (stiffness)7.45GPa285.5GPa111.5x stiffer
Densitynot sourced6,600kg/m³1
Strength to weightnot sourced33.5kN·m/kg
Stiffness to weightnot sourced13MN·m/kg
Poisson's rationot sourced0.273
Shear modulusnot sourced33.7GPa
Bulk modulusnot sourced62GPa
Speed of soundnot sourced3,599m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Zinc Zamak 3
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Zinc Zamak 3
Strength against densityHigher and further left: stronger for its weight
ThermalPlywoodZinc Zamak 3
Thermal conductivity0.12W/m·K4113W/m·K1
Thermal expansionbase material3.1–4.5µm/m·K527.4µm/m·K1
100 mm part over a 50 °C swing19µm growth7.21x less137µm growth
Specific heatbase material1,700J/kg·K54.06x higher419J/kg·K1
Heats up and cools (diffusivity)not sourced40.9mm²/s
Thermal shock resistancenot sourced7,782W/m
Melting pointnot sourcedmelting range381–387°C1
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Zinc Zamak 3
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30PlywoodZinc Zamak 3
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA sample part to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: Nathan Trotter, USDA Forest Products Laboratory, Eastern Alloys
Plywood
Douglas-fir plywood sheathing (construction plywood per PS 1), static bending properties from USDA FPL Wood Handbook FPL-GTR-282 Ch. 12 Table 12-2 (Biblis 2000)
Zinc Zamak 3
Zamak 3 (ASTM B86 die cast), Nathan Trotter (zinc alloy producer) technical data sheet, typical values
  1. 1
    Zamak 3 Technical Data SheetNathan Trotterarchived copyZinc Zamak 3 · Yield strength: typicalZinc Zamak 3 · Ultimate tensile strength: typicalZinc Zamak 3 · Elongation at break: typical, in 2 in.Zinc Zamak 3 · Young's modulus (stiffness): typicalZinc Zamak 3 · Density: typicalZinc Zamak 3 · Thermal conductivity: typicalZinc Zamak 3 · Thermal expansion: typicalZinc Zamak 3 · Specific heat: typicalZinc Zamak 3 · Melting point: melting range
  2. 2
    Wood Handbook (FPL-GTR-282), Chapter 12: Mechanical Properties of Wood-Based Composite MaterialsUSDA Forest Products LaboratoryPlywood · Ultimate tensile strength: modulus of rupture (no direct tensile value)Plywood · Flexural strength: static bending MOR (Douglas-fir); range 33.72-42.61 across speciesPlywood · Young's modulus (stiffness): static bending MOE of the panel (Douglas-fir); range 6.96-8.55 across species
  3. 3
    Zinc Die Casting Properties Guide (2012)Eastern AlloysZinc Zamak 3 · Poisson's ratio: typical, Zamak 3 hot-chamber die cast
  4. 4
    Thermal Properties of Wood and Wood Panel Products for Use in Buildings (1988)USDA Forest Products Laboratoryarchived copyPlywood · Thermal conductivity: APA-recommended design value (Douglas-fir plywood), as reported by FPL/ORNL
  5. 5
    Wood Handbook (FPL-GTR-282), Chapter 4: Moisture Relations and Physical Properties of WoodUSDA Forest Products LaboratoryPlywood · Thermal expansion: base material: solid wood parallel to grain, ovendry, range across speciesPlywood · Specific heat: base material: solid wood (all species), 12% MC, 27 C

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Plywood stronger than Zinc Zamak 3?

Zinc Zamak 3 is stronger: its yield strength is 221 MPa against tensile strength 41.4 MPa for Plywood (5.34x).

Which is stiffer, Plywood or Zinc Zamak 3?

Zinc Zamak 3 is stiffer: Young's modulus 85.5 GPa against 7.45 GPa for Plywood, so the same part in Zinc Zamak 3 deflects less under the same load.

Thermal

Which conducts heat better, Plywood or Zinc Zamak 3?

Zinc Zamak 3 conducts heat better: 113 W/m·K against 0.12 W/m·K for Plywood.

Which expands less with temperature?

Plywood expands less: 3.8 µm/m·K against 27.4 µm/m·K for Zinc Zamak 3.

Related comparisons