Materials / Compare

SLA Resin Standard vs. Titanium Ti-6Al-4V

Compare SLA Resin Standard vs. Titanium Ti-6Al-4V strength, stiffness, weight and thermal properties.

SLA Resin Standard3D printed (SLA resin)
Titanium Ti-6Al-4VWrought
MechanicalSLA Resin StandardTitanium Ti-6Al-4V
Yield strengthnot given (tensile used)885MPa1
Ultimate tensile strength60MPa2940MPa115.7x stronger
Flexural strength105MPa2not sourced
Elongation at break8%216%12x more ductile
Young's modulus (stiffness)2.75GPa2107–122GPa3
Density1,210kg/m³43.66x lighter4,430kg/m³1
Strength to weight49.6kN·m/kg200kN·m/kg4.03x higher
Stiffness to weight2.27MN·m/kg25.8MN·m/kg11.4x higher
Poisson's rationot sourced0.3421
Shear modulusnot sourced42.7GPa
Bulk modulusnot sourced121GPa
Speed of sound1,508m/s5,084m/s3.37x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SLA Resin StandardTitanium Ti-6Al-4V
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SLA Resin StandardTitanium Ti-6Al-4V
Strength against densityHigher and further left: stronger for its weight
ThermalSLA Resin StandardTitanium Ti-6Al-4V
Thermal conductivity0.54W/m·K56.6W/m·K312.2x more heat through a fin
Thermal expansionmean -30 to 140 °C114µm/m·K59µm/m·K312.7x less
100 mm part over a 50 °C swing571µm growth45µm growth12.7x less
Specific heat1,800J/kg·K53.1x higher580J/kg·K3
Heats up and cools (diffusivity)0.248mm²/s2.57mm²/s10.4x faster
Thermal shock resistancenot sourced3,730W/m
Melting pointnot sourcedmelting range1,630–1,650°C1
Max service temperatureHDT 1.8 MPa59°C2400°C1
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SLA Resin StandardTitanium Ti-6Al-4V
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30SLA Resin StandardTitanium Ti-6Al-4V
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: TIMET, Formlabs
SLA Resin Standard
Formlabs Clear Resin V5 (FLGPCL05), TDS Rev. 01 March 20, 2024; printed on Form 4 at 100 µm, washed 5 min in >=99% IPA, post-cured 15 min at 60 °C in Form Cure. Orientation not stated.
Titanium Ti-6Al-4V
TIMETAL 6-4 (Ti-6Al-4V Grade 5) annealed plate typical (TIMET properties manual) + TIMET datasheet TMC-0150 physical properties
  1. 1
    TIMETAL 6-4 PropertiesTIMETarchived copyTitanium Ti-6Al-4V · Yield strength: typical, plate (>0.187 in), annealed, 0.2% offsetTitanium Ti-6Al-4V · Ultimate tensile strength: typical, plate, annealedTitanium Ti-6Al-4V · Elongation at break: typical, in 2 in., plate annealedTitanium Ti-6Al-4V · Density: nominalTitanium Ti-6Al-4V · Poisson's ratio: mean of TIMET measurementsTitanium Ti-6Al-4V · Melting point: melting rangeTitanium Ti-6Al-4V · Max service temperature: upper recommended use temperature
  2. 2
    Clear Resin V5 Technical Data Sheet (2024)Formlabsarchived copySLA Resin Standard · Ultimate tensile strength: typicalSLA Resin Standard · Flexural strength: typicalSLA Resin Standard · Elongation at break: typicalSLA Resin Standard · Young's modulus (stiffness): typicalSLA Resin Standard · Max service temperature: HDT 1.8 MPa
  3. 3
    TIMETAL 6-4 Data SheetTIMETarchived copyTitanium Ti-6Al-4V · Young's modulus (stiffness): typical range, 20 °CTitanium Ti-6Al-4V · Thermal conductivity: typical, 20 °C, mill annealedTitanium Ti-6Al-4V · Thermal expansion: typical, mean 0-100 °CTitanium Ti-6Al-4V · Specific heat: typical, 20 °C
  4. 4
    Clear Resin V5 Technical Data Sheet (web edition)FormlabsSLA Resin Standard · Density: typical, post-cured (same for 5 min ambient and 15 min at 60 °C), ASTM D792
  5. 5
    Thermal Properties of Selected Formlabs SLA ResinsFormlabsSLA Resin Standard · Thermal conductivity: typical, post-cured, ASTM E1530SLA Resin Standard · Thermal expansion: mean -30 to 140 °C, post-cured (5 min ambient cure), TMA ASTM E831SLA Resin Standard · Specific heat: typical, 25 °C, post-cured (5 min ambient cure), DSC ASTM E1269

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

SLA Resin Standard is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is SLA Resin Standard stronger than Titanium Ti-6Al-4V?

Titanium Ti-6Al-4V is stronger: its yield strength is 885 MPa against tensile strength 60 MPa for SLA Resin Standard (14.8x).

Which is lighter, SLA Resin Standard or Titanium Ti-6Al-4V?

SLA Resin Standard is lighter: 1,210 kg/m³ against 4,430 kg/m³ for Titanium Ti-6Al-4V.

Which is stiffer, SLA Resin Standard or Titanium Ti-6Al-4V?

Titanium Ti-6Al-4V is stiffer: Young's modulus 115 GPa against 2.75 GPa for SLA Resin Standard, so the same part in Titanium Ti-6Al-4V deflects less under the same load.

Which is lighter for the same job, SLA Resin Standard or Titanium Ti-6Al-4V?

For the same stiffness or strength: SLA Resin Standard is lighter for a stiff panel or plate; Titanium Ti-6Al-4V is lighter for a stiff rod or tie (tension), stiff beam (bending), strong rod or tie, strong beam, strong panel or plate.

Part that must beSLA Resin StandardTitanium Ti-6Al-4V
Stiff rod or tie (tension)11.4x heavierlighter
Stiff beam (bending)1.76x heavierlighter
Stiff panel or platelighter6% heavier
Strong rod or tie4.03x heavierlighter
Strong beam1.64x heavierlighter
Strong panel or plate5% heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, SLA Resin Standard or Titanium Ti-6Al-4V?

Titanium Ti-6Al-4V stretches further before it breaks: 16% elongation at break against 8% for SLA Resin Standard.

Thermal

Which conducts heat better, SLA Resin Standard or Titanium Ti-6Al-4V?

Titanium Ti-6Al-4V conducts heat better: 6.6 W/m·K against 0.54 W/m·K for SLA Resin Standard.

Which expands less with temperature?

Titanium Ti-6Al-4V expands less: 9 µm/m·K against 114 µm/m·K for SLA Resin Standard.