Materials / Stainless Steel

Stainless Steel 304

Stainless Steel 304 strength, stiffness, density and thermal properties, with their source.

A bracket in Stainless Steel 304, brushed finish.

ProcessWrought
Mechanical
Yield strength241MPasourcetypical, annealed, 70 °F (21 °C)
Ultimate tensile strength586MPasourcetypical, annealed, 70 °F (21 °C)
Elongation at break55%sourcetypical, annealed, in 2 in. (50.8 mm)
Young's modulus (stiffness)193GPasourcetypical, in tension
Density8,030kg/m³sourcetypical
Strength to weight30kN·m/kg
Stiffness to weight24MN·m/kg
Poisson's ratio0.3sourcedesign value (structural stainless steels)
Shear modulus74.2GPa
Bulk modulus161GPa
Speed of sound4,903m/s
Thermal
Thermal conductivity16.2W/m·Ksourceat 100 °C
Thermal expansion16.9µm/m·Ksourcemean, 0–100 °C
100 mm part over a 50 °C swing84.5µm growth
Specific heat500J/kg·Ksourcemean, 0–100 °C
Heats up and cools (diffusivity)4.03mm²/s
Thermal shock resistance838W/m
Melting point1,399–1,454°Csourcemelting range
Max service temperature899°Csourcecontinuous, oxidation (scaling) limit in air
Values forType 304, annealed flat-rolled (Cleveland-Cliffs 304/304L Product Data Bulletin, May 2021); Poisson's ratio from the Nickel Institute/SCI structural stainless design manual

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelStainless Steel 304
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickStainless Steel 304
Strength against density

Compare Stainless Steel 304 with