Materials / Compare

Aluminum 2024-T351 vs. Stainless Steel 304

Compare Aluminum 2024-T351 vs. Stainless Steel 304 strength, stiffness, weight and thermal properties.

Aluminum 2024-T351Wrought
Stainless Steel 304Wrought
MechanicalAluminum 2024-T351Stainless Steel 304
Yield strength324MPa134% stronger241MPa2
Ultimate tensile strength469MPa1586MPa225% stronger
Elongation at break19%155%22.89x more ductile
Young's modulus (stiffness)73.1GPa1193GPa22.64x stiffer
Density2,770kg/m³12.9x lighter8,030kg/m³2
Strength to weight117kN·m/kg3.9x higher30kN·m/kg
Stiffness to weight26.4MN·m/kg10% higher24MN·m/kg
Poisson's ratio0.333design value0.34
Shear modulus27.5GPa74.2GPa2.7x stiffer in shear
Bulk modulus71.7GPa161GPa2.24x higher
Speed of sound5,137m/s5% faster4,903m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 2024-T351Stainless Steel 304
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 2024-T351Stainless Steel 304
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 2024-T351Stainless Steel 304
Thermal conductivity120W/m·K17.41x more heat through a finat 100 °C16.2W/m·K2
Thermal expansion22.9µm/m·K1mean16.9µm/m·K236% less
100 mm part over a 50 °C swing115µm growth84.5µm growth36% less
Specific heat875J/kg·K11.75x highermean500J/kg·K2
Heats up and cools (diffusivity)49.5mm²/s12.3x faster4.03mm²/s
Thermal shock resistance15,561W/m18.6x more resistant838W/m
Melting pointmelting range502–638°C1melting range1,399–1,454°C2
Max service temperaturenot sourcedcontinuous899°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 2024-T351Stainless Steel 304
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 2024-T351Stainless Steel 304
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Kaiser Aluminum, Cleveland-Cliffs, U.S. Department of Defense, Steel Construction Institute
Aluminum 2024-T351
2024-T4/T351, Kaiser Aluminum sheet, coil & plate typical datasheet; Poisson from MIL-HDBK-5J
Stainless Steel 304
Type 304, annealed flat-rolled (Cleveland-Cliffs 304/304L Product Data Bulletin, May 2021); Poisson's ratio from the Nickel Institute/SCI structural stainless design manual
  1. 1
    Alloy 2024 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 2024-T351 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 2024-T351 · Ultimate tensile strength: typicalAluminum 2024-T351 · Elongation at break: typical, in 4DAluminum 2024-T351 · Young's modulus (stiffness): typicalAluminum 2024-T351 · Density: nominalAluminum 2024-T351 · Thermal conductivity: typical, 20 °CAluminum 2024-T351 · Thermal expansion: typical, mean 20-100 °CAluminum 2024-T351 · Specific heat: typical, at 100 °CAluminum 2024-T351 · Melting point: melting range
  2. 2
    304/304L Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsStainless Steel 304 · Yield strength: typical, annealed, 70 °F (21 °C)Stainless Steel 304 · Ultimate tensile strength: typical, annealed, 70 °F (21 °C)Stainless Steel 304 · Elongation at break: typical, annealed, in 2 in. (50.8 mm)Stainless Steel 304 · Young's modulus (stiffness): typical, in tensionStainless Steel 304 · Density: typicalStainless Steel 304 · Thermal conductivity: at 100 °CStainless Steel 304 · Thermal expansion: mean, 0–100 °CStainless Steel 304 · Specific heat: mean, 0–100 °CStainless Steel 304 · Melting point: melting rangeStainless Steel 304 · Max service temperature: continuous, oxidation (scaling) limit in air
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 2024-T351 · Poisson's ratio: typical (handbook physical constant), all tempers
  4. 4
    Design Manual for Structural Stainless Steel, 4th Edition (P413)Steel Construction Institutearchived copyStainless Steel 304 · Poisson's ratio: design value (structural stainless steels)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 2024-T351 stronger than Stainless Steel 304?

Aluminum 2024-T351 is stronger: its yield strength is 324 MPa against 241 MPa for Stainless Steel 304 (34%).

Which is lighter, Aluminum 2024-T351 or Stainless Steel 304?

Aluminum 2024-T351 is lighter: 2,770 kg/m³ against 8,030 kg/m³ for Stainless Steel 304.

Which is stiffer, Aluminum 2024-T351 or Stainless Steel 304?

Stainless Steel 304 is stiffer: Young's modulus 193 GPa against 73.1 GPa for Aluminum 2024-T351, so the same part in Stainless Steel 304 deflects less under the same load.

Which is lighter for the same job, Aluminum 2024-T351 or Stainless Steel 304?

For the same stiffness or strength: Aluminum 2024-T351 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 2024-T351Stainless Steel 304
Stiff rod or tie (tension)lighter10% heavier
Stiff beam (bending)lighter1.78x heavier
Stiff panel or platelighter2.1x heavier
Strong rod or tielighter3.9x heavier
Strong beamlighter3.53x heavier
Strong panel or platelighter3.36x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 2024-T351 or Stainless Steel 304?

Stainless Steel 304 stretches further before it breaks: 55% elongation at break against 19% for Aluminum 2024-T351.

Thermal

Which conducts heat better, Aluminum 2024-T351 or Stainless Steel 304?

Aluminum 2024-T351 conducts heat better: 120 W/m·K against 16.2 W/m·K for Stainless Steel 304.

Which expands less with temperature?

Stainless Steel 304 expands less: 16.9 µm/m·K against 22.9 µm/m·K for Aluminum 2024-T351.

Related comparisons