Materials / Compare
Aluminum 2024-T351 vs. Steel AISI 1045 Compare Aluminum 2024-T351 vs. Steel AISI 1045 strength, stiffness, weight and thermal properties.
Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless Steel 304 Stainless Steel 316 Stainless Steel 303 Stainless Steel 17-4PH Brass C360 Brass C260 Copper C110 Copper C10100 Copper C12200 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Magnesium AZ91D Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall PCB Laminate FR-4 PCB Board FR-4, 2 copper planes Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Solder SAC305 Aluminum 2024-T351 Wrought Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless Steel 304 Stainless Steel 316 Stainless Steel 303 Stainless Steel 17-4PH Brass C360 Brass C260 Copper C110 Copper C10100 Copper C12200 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Magnesium AZ91D Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall PCB Laminate FR-4 PCB Board FR-4, 2 copper planes Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Solder SAC305 Steel AISI 1045 Wrought Mechanical Aluminum 2024-T351 Steel AISI 1045 Yield strength 324 MPa producer-stated 531 MPa 1.64x stronger Ultimate tensile strength 469 MPa producer-stated 627 MPa 34% stronger Elongation at break 19 % 1.58x more ductile in 2 in 12 % Young's modulus (stiffness) 73.1 GPa 210 GPa 2.87x stiffer Density 2,770 kg/m³ 2.82x lighter 7,800 kg/m³ Strength to weight 117 kN·m/kg 1.72x higher 68.1 kN·m/kg Stiffness to weight 26.4 MN·m/kg 26.9 MN·m/kg 2% higher Poisson's ratio 0.33 0.3 Shear modulus 27.5 GPa 80.8 GPa 2.94x stiffer in shear Bulk modulus 71.7 GPa 175 GPa 2.44x higher Speed of sound 5,137 m/s 5,189 m/s
1k 10k 0.1 1 10 100 Density (kg/m³) Young's modulus (GPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum 2024-T351 Steel AISI 1045 Stiffness against densityHigher and further left: stiffer for its weight 1k 10k 10 100 1k Density (kg/m³) Yield strength (MPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Rubber Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Brick PCB Laminate FR-4 Silicon Ceramic Alumina 96% Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum 2024-T351 Steel AISI 1045 Strength against densityHigher and further left: stronger for its weight
Thermal Aluminum 2024-T351 Steel AISI 1045 Thermal conductivity 120 W/m·K 40–45 W/m·K Thermal expansion 22.9 µm/m·K 12 µm/m·K 1.91x less 100 mm part over a 50 °C swing 115 µm growth 60 µm growth 1.91x less Specific heat 875 J/kg·K 460–480 J/kg·K Heats up and cools (diffusivity) 49.5 mm²/s 4.27x faster 11.6 mm²/s Thermal shock resistance 15,561 W/m 2.48x more resistant 6,269 W/m Melting point melting range 502–638 °C not sourced
1k 10k 0.1 1 10 100 Density (kg/m³) Thermal conductivity (W/m·K) Plastic PLA Plastic PETG Plastic ABS Plastic Nylon Rubber Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM HIPS SLA Resin Standard DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum 2024-T351 Steel AISI 1045 Thermal conductivity against densityHigher and further left: spreads more heat for its weight 0.1 1 10 100 10 100 Thermal conductivity (W/m·K) Thermal expansion (µm/m·K) Plastic PETG Plastic ABS Plastic Nylon Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM HIPS SLA Resin Standard DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum 2024-T351 Steel AISI 1045 Thermal expansion against thermal conductivityLower and further right: warps less when heated
Sources 4 documents: Kaiser Aluminum, Niagara LaSalle, Ovako, U.S. Department of Defense
Aluminum 2024-T351 2024-T4/T351, Kaiser Aluminum sheet, coil & plate typical datasheet; Poisson from MIL-HDBK-5J
Steel AISI 1045 AISI 1045 cold drawn bar (Niagara LaSalle) for mechanical; Ovako C45 (lists 'SAE 1045' as a similar designation) for physical constants 1 Alloy 2024 Sheet, Coil & Plate Technical Data Kaiser Aluminum archived copy Aluminum 2024-T351 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 2024-T351 · Ultimate tensile strength: typicalAluminum 2024-T351 · Elongation at break: typical, in 4DAluminum 2024-T351 · Young's modulus (stiffness): typicalAluminum 2024-T351 · Density: nominalAluminum 2024-T351 · Thermal conductivity: typical, 20 °CAluminum 2024-T351 · Thermal expansion: typical, mean 20-100 °CAluminum 2024-T351 · Specific heat: typical, at 100 °CAluminum 2024-T351 · Melting point: melting range2 1045 Properties Niagara LaSalle archived copy Steel AISI 1045 · Yield strength: producer-stated, cold drawnSteel AISI 1045 · Ultimate tensile strength: producer-stated, cold drawnSteel AISI 1045 · Elongation at break: in 2 in (50.8 mm)3 C45 Steel Grade Ovako Steel AISI 1045 · Young's modulus (stiffness): typicalSteel AISI 1045 · Density: typicalSteel AISI 1045 · Poisson's ratio: typicalSteel AISI 1045 · Thermal conductivity: typical range, ambientSteel AISI 1045 · Thermal expansion: typical, mean 20-300 °CSteel AISI 1045 · Specific heat: typical range, 50/100 °C
4 MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003) U.S. Department of Defense Aluminum 2024-T351 · Poisson's ratio: typical (handbook physical constant), all tempers
Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
Questions Mechanical Is Aluminum 2024-T351 stronger than Steel AISI 1045? Steel AISI 1045 is stronger: its yield strength is 531 MPa against 324 MPa for Aluminum 2024-T351 (1.64x).
Which is lighter, Aluminum 2024-T351 or Steel AISI 1045? Aluminum 2024-T351 is lighter: 2,770 kg/m³ against 7,800 kg/m³ for Steel AISI 1045.
Which is stiffer, Aluminum 2024-T351 or Steel AISI 1045? Steel AISI 1045 is stiffer: Young's modulus 210 GPa against 73.1 GPa for Aluminum 2024-T351, so the same part in Steel AISI 1045 deflects less under the same load.
Which is lighter for the same job, Aluminum 2024-T351 or Steel AISI 1045? For the same stiffness or strength: Aluminum 2024-T351 is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate; Steel AISI 1045 is lighter for a stiff rod or tie (tension).
Part that must be Aluminum 2024-T351 Steel AISI 1045 Stiff rod or tie (tension) 2% heavier lighter Stiff beam (bending) lighter 1.66x heavier Stiff panel or plate lighter 1.98x heavier Strong rod or tie lighter 1.72x heavier Strong beam lighter 2.03x heavier Strong panel or plate lighter 2.2x heavier
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Which is more ductile, Aluminum 2024-T351 or Steel AISI 1045? Aluminum 2024-T351 stretches further before it breaks: 19% elongation at break against 12% for Steel AISI 1045.
Thermal Which conducts heat better, Aluminum 2024-T351 or Steel AISI 1045? Aluminum 2024-T351 conducts heat better: 120 W/m·K against 42.5 W/m·K for Steel AISI 1045.
Which expands less with temperature? Steel AISI 1045 expands less: 12 µm/m·K against 22.9 µm/m·K for Aluminum 2024-T351.