Materials / Compare

Aluminum 5052-H32 vs. Plastic PETG

Compare Aluminum 5052-H32 vs. Plastic PETG strength, stiffness, weight and thermal properties.

Aluminum 5052-H32Wrought
Plastic PETG3D printed (FDM)
MechanicalAluminum 5052-H32Plastic PETG
Yield strength195MPa14.22x stronger46.2MPa2
Ultimate tensile strength230MPa14.98x stronger46.2MPa2
Flexural strengthnot sourced78.9MPa2
Elongation at break12%11.58x more ductile7.6%2
Young's modulus (stiffness)70GPa136.1x stiffer1.94GPa2
Density2,685kg/m³31,270kg/m³22.11x lighter
Strength to weight72.6kN·m/kg2x higher36.4kN·m/kg
Stiffness to weight26.1MN·m/kg17.1x higher1.53MN·m/kg
Poisson's ratio0.333not sourced
Shear modulus26.3GPanot sourced
Bulk modulus68.6GPanot sourced
Speed of sound5,106m/s4.13x faster1,236m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Plastic PETG
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Plastic PETG
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 5052-H32Plastic PETG
Thermal conductivitybase material138W/m·K1657x more heat through a finbase material0.21W/m·K4
Thermal expansion23.8µm/m·K12.14x lessbase material51µm/m·K4
100 mm part over a 50 °C swing119µm growth2.14x less255µm growth
Specific heatat 100 °C963J/kg·K3base material1,300J/kg·K435% higher
Heats up and cools (diffusivity)53.4mm²/s420x faster0.127mm²/s
Thermal shock resistance10,822W/mnot sourced
Melting pointmelting range605–650°C1not sourced
Glass transitionnot sourced77.4°C2
Max service temperaturenot sourcedHDT 0.455 MPa76.2°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Plastic PETG
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 5052-H32Plastic PETG
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Kaiser Aluminum, UltiMaker, U.S. Department of Defense, Eastman
Aluminum 5052-H32
5052-H32, Kaiser Aluminum tube & pipe typical datasheet (mechanical, CTE, melting); MIL-HDBK-5J (Poisson, density, specific heat)
Plastic PETG
Ultimaker PETG, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS v1.00, April 29, 2022.
  1. 1
    Alloy 5052 Tube & Pipe Technical DataKaiser Aluminumarchived copyAluminum 5052-H32 · Yield strength: typical, 0.2% offsetAluminum 5052-H32 · Ultimate tensile strength: typicalAluminum 5052-H32 · Elongation at break: typicalAluminum 5052-H32 · Young's modulus (stiffness): typicalAluminum 5052-H32 · Thermal conductivity: base material: 5052 in O temper (same alloy, annealed); Kaiser typicalAluminum 5052-H32 · Thermal expansion: typical, mean 20-100 °CAluminum 5052-H32 · Melting point: melting range
  2. 2
    Ultimaker PETG Technical Data Sheet, v1.00UltiMakerarchived copyPlastic PETG · Yield strength: typicalPlastic PETG · Ultimate tensile strength: typical, peak stress (= stress at yield)Plastic PETG · Flexural strength: typicalPlastic PETG · Elongation at break: typicalPlastic PETG · Young's modulus (stiffness): typicalPlastic PETG · Density: typicalPlastic PETG · Glass transition: typicalPlastic PETG · Max service temperature: HDT 0.455 MPa (printed specimens)
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 5052-H32 · Density: nominalAluminum 5052-H32 · Poisson's ratio: typical (handbook physical constant)Aluminum 5052-H32 · Specific heat: at 100 °C (212 °F); table covers O, H32, H34, H36, H38
  4. 4
    Eastar Copolyester 6763 Product Data SheetEastmanPlastic PETG · Thermal conductivity: base material: Eastman Eastar Copolyester 6763 (PETG), typicalPlastic PETG · Thermal expansion: base material: Eastman Eastar Copolyester 6763 (PETG), typicalPlastic PETG · Specific heat: base material: Eastman Eastar Copolyester 6763 (PETG), DSC at 60 °C (lowest temperature listed)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Plastic PETG is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Aluminum 5052-H32 stronger than Plastic PETG?

Aluminum 5052-H32 is stronger: its yield strength is 195 MPa against 46.2 MPa for Plastic PETG (4.22x).

Which is lighter, Aluminum 5052-H32 or Plastic PETG?

Plastic PETG is lighter: 1,270 kg/m³ against 2,685 kg/m³ for Aluminum 5052-H32.

Which is stiffer, Aluminum 5052-H32 or Plastic PETG?

Aluminum 5052-H32 is stiffer: Young's modulus 70 GPa against 1.94 GPa for Plastic PETG, so the same part in Aluminum 5052-H32 deflects less under the same load.

Which is lighter for the same job, Aluminum 5052-H32 or Plastic PETG?

For the same stiffness or strength: Aluminum 5052-H32 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam; Plastic PETG is lighter for a strong panel or plate.

Part that must beAluminum 5052-H32Plastic PETG
Stiff rod or tie (tension)lighter17.1x heavier
Stiff beam (bending)lighter2.84x heavier
Stiff panel or platelighter1.56x heavier
Strong rod or tielighter2x heavier
Strong beamlighter24% heavier
Strong panel or plate3% heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 5052-H32 or Plastic PETG?

Aluminum 5052-H32 stretches further before it breaks: 12% elongation at break against 7.6% for Plastic PETG.

Thermal

Which conducts heat better, Aluminum 5052-H32 or Plastic PETG?

Aluminum 5052-H32 conducts heat better: 138 W/m·K against 0.21 W/m·K for Plastic PETG.

Which expands less with temperature?

Aluminum 5052-H32 expands less: 23.8 µm/m·K against 51 µm/m·K for Plastic PETG.

Related comparisons