Materials / Plastic

Plastic PETG

Plastic PETG strength, stiffness, density and thermal properties, with their source.

A bracket in Plastic PETG, 3D-printed (layer lines) finish.

Process3D printed (FDM)
Mechanical
Yield strength46.2MPasourcetypical
Ultimate tensile strength46.2MPasourcetypical, peak stress (= stress at yield)
Flexural strength78.9MPasourcetypical
Elongation at break7.6%sourcetypical
Young's modulus (stiffness)1.94GPasourcetypical
Density1,270kg/m³sourcetypical
Strength to weight36.4kN·m/kg
Stiffness to weight1.53MN·m/kg
Poisson's rationot sourced
Shear modulusnot sourced
Bulk modulusnot sourced
Speed of sound1,236m/s
Thermal
Thermal conductivity0.21W/m·Ksourcebase material: Eastman Eastar Copolyester 6763 (PETG), typical
Thermal expansion51µm/m·Ksourcebase material: Eastman Eastar Copolyester 6763 (PETG), typical
100 mm part over a 50 °C swing255µm growth
Specific heat1,300J/kg·Ksourcebase material: Eastman Eastar Copolyester 6763 (PETG), DSC at 60 °C (lowest temperature listed)
Heats up and cools (diffusivity)0.127mm²/s
Thermal shock resistancenot sourced
Glass transition77.4°Csourcetypical
Max service temperature76.2°CsourceHDT 0.455 MPa (printed specimens)
Values forUltimaker PETG, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS v1.00, April 29, 2022.

Plastic PETG is 3D printed: its properties depend on build direction and print settings; these are typical values.

Among 59 materials

1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic ABSPlastic TPUPlastic NylonAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelPlastic PETG
Stiffness against density
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic ABSPlastic TPUPlastic NylonRubberAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPlastic PETG
Strength against density

Compare Plastic PETG with