Aluminum 6061-T6 vs. DMLS 17-4PH Stainless Steel

Compare Aluminum 6061-T6 vs. DMLS 17-4PH Stainless Steel strength, stiffness, weight and thermal properties.

Aluminum 6061-T6Wrought
DMLS 17-4PH Stainless Steel3D printed metal (DMLS)
MechanicalAluminum 6061-T6DMLS 17-4PH Stainless Steel
Yield strength276MPa1mean861MPa23.12x stronger
Ultimate tensile strength310MPa1mean886MPa22.86x stronger
Elongation at break17%1mean at break19.9%217% more ductile
Young's modulus (stiffness)68.3GPa1base material197GPa32.88x stiffer
Density2,700kg/m³12.89x lightermean part density7,790kg/m³2
Strength to weight102kN·m/kg110kN·m/kg8% higher
Stiffness to weight25.3MN·m/kg25.3MN·m/kg
Poisson's ratio0.334base material0.2723
Shear modulus25.7GPa77.4GPa3.02x stiffer in shear
Bulk modulus67GPa144GPa2.15x higher
Speed of sound5,030m/s5,029m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6DMLS 17-4PH Stainless Steel
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6DMLS 17-4PH Stainless Steel
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 6061-T6DMLS 17-4PH Stainless Steel
Thermal conductivity167W/m·K19.33x more heat through a finbase material17.9W/m·K3
Thermal expansion23.6µm/m·K1mean 25-100 °C10.4µm/m·K22.27x less
100 mm part over a 50 °C swing118µm growth52µm growth2.27x less
Specific heat896J/kg·K11.95x higherbase material460J/kg·K3
Heats up and cools (diffusivity)69mm²/s13.8x faster5mm²/s
Thermal shock resistance19,159W/m3.5x more resistant5,474W/m
Melting pointsolidus-liquidus582–652°C1not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6DMLS 17-4PH Stainless Steel
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6DMLS 17-4PH Stainless Steel
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Kaiser Aluminum, EOS GmbH, Cleveland-Cliffs, U.S. Department of Defense
Aluminum 6061-T6
6061-T6/T651, Kaiser Aluminum typical properties; Poisson from MIL-HDBK-5J
DMLS 17-4PH Stainless Steel
EOS StainlessSteel 17-4PH IndustryLine (powder 9011-0041), EOS M 290, 40 µm, default job 17-4PH_040_StainlessM291_100, as built, horizontal; ISO 6892 & ASTM E8M
  1. 1
    Alloy 6061 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 6061-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 6061-T6 · Ultimate tensile strength: typicalAluminum 6061-T6 · Elongation at break: typical, in 4D, 0.500 in dia specimenAluminum 6061-T6 · Young's modulus (stiffness): typicalAluminum 6061-T6 · Density: nominalAluminum 6061-T6 · Thermal conductivity: typical, 20 °CAluminum 6061-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 6061-T6 · Specific heat: typical, at 100 °CAluminum 6061-T6 · Melting point: solidus-liquidus
  2. 2
    EOS StainlessSteel 17-4PH IndustryLine Material Data Sheet, M 290EOS GmbHarchived copyDMLS 17-4PH Stainless Steel · Yield strength: mean, as built, horizontal (N=72)DMLS 17-4PH Stainless Steel · Ultimate tensile strength: mean, as built, horizontal (N=72)DMLS 17-4PH Stainless Steel · Elongation at break: mean at break, as built, horizontalDMLS 17-4PH Stainless Steel · Density: mean part density (ISO 3369)DMLS 17-4PH Stainless Steel · Thermal expansion: mean 25-100 °C, ASTM E228, AFTER atmospheric heat treatment (as-built value not published)
  3. 3
    17-4 PH Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsDMLS 17-4PH Stainless Steel · Young's modulus (stiffness): base material: wrought 17-4 PH, Condition H 900 (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Poisson's ratio: base material: wrought 17-4 PH, all conditions (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Thermal conductivity: base material: wrought 17-4 PH, Condition H 900, at 149 °C (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Specific heat: base material: wrought 17-4 PH, Condition A, 0-100 °C (Cleveland-Cliffs)
  4. 4
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 6061-T6 · Poisson's ratio: typical (handbook physical constant)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

DMLS 17-4PH Stainless Steel is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Aluminum 6061-T6 stronger than DMLS 17-4PH Stainless Steel?

DMLS 17-4PH Stainless Steel is stronger: its yield strength is 861 MPa against 276 MPa for Aluminum 6061-T6 (3.12x).

Which is lighter, Aluminum 6061-T6 or DMLS 17-4PH Stainless Steel?

Aluminum 6061-T6 is lighter: 2,700 kg/m³ against 7,790 kg/m³ for DMLS 17-4PH Stainless Steel.

Which is stiffer, Aluminum 6061-T6 or DMLS 17-4PH Stainless Steel?

DMLS 17-4PH Stainless Steel is stiffer: Young's modulus 197 GPa against 68.3 GPa for Aluminum 6061-T6, so the same part in DMLS 17-4PH Stainless Steel deflects less under the same load.

Which is lighter for the same job, Aluminum 6061-T6 or DMLS 17-4PH Stainless Steel?

For the same stiffness or strength: Aluminum 6061-T6 is lighter for a stiff beam (bending), stiff panel or plate, strong beam, strong panel or plate; DMLS 17-4PH Stainless Steel is lighter for a strong rod or tie.

Part that must beAluminum 6061-T6DMLS 17-4PH Stainless Steel
Stiff rod or tie (tension)about equalabout equal
Stiff beam (bending)lighter1.7x heavier
Stiff panel or platelighter2.03x heavier
Strong rod or tie8% heavierlighter
Strong beamlighter35% heavier
Strong panel or platelighter1.63x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 6061-T6 or DMLS 17-4PH Stainless Steel?

DMLS 17-4PH Stainless Steel stretches further before it breaks: 19.9% elongation at break against 17% for Aluminum 6061-T6.

Thermal

Which conducts heat better, Aluminum 6061-T6 or DMLS 17-4PH Stainless Steel?

Aluminum 6061-T6 conducts heat better: 167 W/m·K against 17.9 W/m·K for DMLS 17-4PH Stainless Steel.

Which expands less with temperature?

DMLS 17-4PH Stainless Steel expands less: 10.4 µm/m·K against 23.6 µm/m·K for Aluminum 6061-T6.