Thermal conductivity against densityHigher and further left: spreads more heat for its weightThermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browser
Sources4 documents: Kaiser Aluminum, LyondellBasell, U.S. Department of Defense, INEOS Olefins & Polymers USA
Aluminum 6061-T6
6061-T6/T651, Kaiser Aluminum typical properties; Poisson from MIL-HDBK-5J
Plastic HDPE
LyondellBasell Hostalen 23050 B high density polyethylene, typical ISO values
1
Alloy 6061 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 6061-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 6061-T6 · Ultimate tensile strength: typicalAluminum 6061-T6 · Elongation at break: typical, in 4D, 0.500 in dia specimenAluminum 6061-T6 · Young's modulus (stiffness): typicalAluminum 6061-T6 · Density: nominalAluminum 6061-T6 · Thermal conductivity: typical, 20 °CAluminum 6061-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 6061-T6 · Specific heat: typical, at 100 °CAluminum 6061-T6 · Melting point: solidus-liquidus
2
Hostalen 23050 B Product DataLyondellBasellPlastic HDPE · Yield strength: typical, tensile stress at yield 23 °C, 50 mm/min ISO 527Plastic HDPE · Young's modulus (stiffness): typical, tensile modulus 23 °C ISO 527Plastic HDPE · Density: typical, ISO 1183
3
MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 6061-T6 · Poisson's ratio: typical (handbook physical constant)
4
Typical Engineering Properties of High Density PolyethyleneINEOS Olefins & Polymers USAarchived copyPlastic HDPE · Poisson's ratio: base material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)Plastic HDPE · Thermal conductivity: base material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)Plastic HDPE · Thermal expansion: base material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)Plastic HDPE · Specific heat: base material: high-density polyethylene family (INEOS Olefins & Polymers USA, Typical Engineering Properties of HDPE)
Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
Questions
Mechanical
Is Aluminum 6061-T6 stronger than Plastic HDPE?
Aluminum 6061-T6 is stronger: its yield strength is 276 MPa against 24 MPa for Plastic HDPE (11.5x).
Which is lighter, Aluminum 6061-T6 or Plastic HDPE?
Plastic HDPE is lighter: 950 kg/m³ against 2,700 kg/m³ for Aluminum 6061-T6.
Which is stiffer, Aluminum 6061-T6 or Plastic HDPE?
Aluminum 6061-T6 is stiffer: Young's modulus 68.3 GPa against 0.9 GPa for Plastic HDPE, so the same part in Aluminum 6061-T6 deflects less under the same load.
Which is lighter for the same job, Aluminum 6061-T6 or Plastic HDPE?
For the same stiffness or strength: Aluminum 6061-T6 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.
Part that must be
Aluminum 6061-T6
Plastic HDPE
Stiff rod or tie (tension)
lighter
26.7x heavier
Stiff beam (bending)
lighter
3.07x heavier
Stiff panel or plate
lighter
49% heavier
Strong rod or tie
lighter
4.05x heavier
Strong beam
lighter
1.79x heavier
Strong panel or plate
lighter
19% heavier
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Thermal
Which conducts heat better, Aluminum 6061-T6 or Plastic HDPE?
Aluminum 6061-T6 conducts heat better: 167 W/m·K against 0.445 W/m·K for Plastic HDPE.
Which expands less with temperature?
Aluminum 6061-T6 expands less: 23.6 µm/m·K against 120 µm/m·K for Plastic HDPE.