Thermal conductivity against densityHigher and further left: spreads more heat for its weightThermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browser
Sources3 documents: Kaiser Aluminum, Cleveland-Cliffs, U.S. Department of Defense
Aluminum 6061-T6
6061-T6/T651, Kaiser Aluminum typical properties; Poisson from MIL-HDBK-5J
Stainless Steel 17-4PH
Cleveland-Cliffs 17-4 PH, Condition H 900, sheet/strip, transverse (Product Data Bulletin, May 2021)
1
Alloy 6061 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 6061-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 6061-T6 · Ultimate tensile strength: typicalAluminum 6061-T6 · Elongation at break: typical, in 4D, 0.500 in dia specimenAluminum 6061-T6 · Young's modulus (stiffness): typicalAluminum 6061-T6 · Density: nominalAluminum 6061-T6 · Thermal conductivity: typical, 20 °CAluminum 6061-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 6061-T6 · Specific heat: typical, at 100 °CAluminum 6061-T6 · Melting point: solidus-liquidus
2
17-4 PH Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsStainless Steel 17-4PH · Yield strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Ultimate tensile strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Elongation at break: typical, transverse, in 2 in. (50.8 mm)Stainless Steel 17-4PH · Young's modulus (stiffness): H 900Stainless Steel 17-4PH · Density: H 900Stainless Steel 17-4PH · Poisson's ratio: H 900 (column)Stainless Steel 17-4PH · Thermal conductivity: at 149 °C (300 °F), H 900Stainless Steel 17-4PH · Thermal expansion: mean, 21–93 °C (70–200 °F), H 900Stainless Steel 17-4PH · Specific heat: mean, 0–100 °C, H 900Stainless Steel 17-4PH · Max service temperature: strength-retention limit (not oxidation)
3
MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 6061-T6 · Poisson's ratio: typical (handbook physical constant)
Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
Questions
Mechanical
Is Aluminum 6061-T6 stronger than Stainless Steel 17-4PH?
Stainless Steel 17-4PH is stronger: its yield strength is 1,275 MPa against 276 MPa for Aluminum 6061-T6 (4.62x).
Which is lighter, Aluminum 6061-T6 or Stainless Steel 17-4PH?
Aluminum 6061-T6 is lighter: 2,700 kg/m³ against 7,800 kg/m³ for Stainless Steel 17-4PH.
Which is stiffer, Aluminum 6061-T6 or Stainless Steel 17-4PH?
Stainless Steel 17-4PH is stiffer: Young's modulus 197 GPa against 68.3 GPa for Aluminum 6061-T6, so the same part in Stainless Steel 17-4PH deflects less under the same load.
Which is lighter for the same job, Aluminum 6061-T6 or Stainless Steel 17-4PH?
For the same stiffness or strength: Aluminum 6061-T6 is lighter for a stiff beam (bending), stiff panel or plate, strong beam, strong panel or plate; Stainless Steel 17-4PH is lighter for a strong rod or tie.
Part that must be
Aluminum 6061-T6
Stainless Steel 17-4PH
Stiff rod or tie (tension)
about equal
about equal
Stiff beam (bending)
lighter
1.7x heavier
Stiff panel or plate
lighter
2.03x heavier
Strong rod or tie
1.6x heavier
lighter
Strong beam
lighter
4% heavier
Strong panel or plate
lighter
34% heavier
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Which is more ductile, Aluminum 6061-T6 or Stainless Steel 17-4PH?
Aluminum 6061-T6 stretches further before it breaks: 17% elongation at break against 9% for Stainless Steel 17-4PH.
Thermal
Which conducts heat better, Aluminum 6061-T6 or Stainless Steel 17-4PH?
Aluminum 6061-T6 conducts heat better: 167 W/m·K against 17.9 W/m·K for Stainless Steel 17-4PH.
Which expands less with temperature?
Stainless Steel 17-4PH expands less: 10.8 µm/m·K against 23.6 µm/m·K for Aluminum 6061-T6.