Materials / Compare

Aluminum 6061-T6 vs. Steel AISI 1045

Compare Aluminum 6061-T6 vs. Steel AISI 1045 strength, stiffness, weight and thermal properties.

Aluminum 6061-T6Wrought
Steel AISI 1045Wrought
MechanicalAluminum 6061-T6Steel AISI 1045
Yield strength276MPa1producer-stated531MPa21.92x stronger
Ultimate tensile strength310MPa1producer-stated627MPa22.02x stronger
Elongation at break17%142% more ductilein 2 in12%2
Young's modulus (stiffness)68.3GPa1210GPa33.07x stiffer
Density2,700kg/m³12.89x lighter7,800kg/m³3
Strength to weight102kN·m/kg1.5x higher68.1kN·m/kg
Stiffness to weight25.3MN·m/kg26.9MN·m/kg6% higher
Poisson's ratio0.3340.33
Shear modulus25.7GPa80.8GPa3.15x stiffer in shear
Bulk modulus67GPa175GPa2.61x higher
Speed of sound5,030m/s5,189m/s3% faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6Steel AISI 1045
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6Steel AISI 1045
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 6061-T6Steel AISI 1045
Thermal conductivity167W/m·K140–45W/m·K3
Thermal expansion23.6µm/m·K112µm/m·K31.97x less
100 mm part over a 50 °C swing118µm growth60µm growth1.97x less
Specific heat896J/kg·K1460–480J/kg·K3
Heats up and cools (diffusivity)69mm²/s5.95x faster11.6mm²/s
Thermal shock resistance19,159W/m3.06x more resistant6,269W/m
Melting pointsolidus-liquidus582–652°C1not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6Steel AISI 1045
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6Steel AISI 1045
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Kaiser Aluminum, Niagara LaSalle, Ovako, U.S. Department of Defense
Aluminum 6061-T6
6061-T6/T651, Kaiser Aluminum typical properties; Poisson from MIL-HDBK-5J
Steel AISI 1045
AISI 1045 cold drawn bar (Niagara LaSalle) for mechanical; Ovako C45 (lists 'SAE 1045' as a similar designation) for physical constants
  1. 1
    Alloy 6061 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 6061-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 6061-T6 · Ultimate tensile strength: typicalAluminum 6061-T6 · Elongation at break: typical, in 4D, 0.500 in dia specimenAluminum 6061-T6 · Young's modulus (stiffness): typicalAluminum 6061-T6 · Density: nominalAluminum 6061-T6 · Thermal conductivity: typical, 20 °CAluminum 6061-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 6061-T6 · Specific heat: typical, at 100 °CAluminum 6061-T6 · Melting point: solidus-liquidus
  2. 2
    1045 PropertiesNiagara LaSallearchived copySteel AISI 1045 · Yield strength: producer-stated, cold drawnSteel AISI 1045 · Ultimate tensile strength: producer-stated, cold drawnSteel AISI 1045 · Elongation at break: in 2 in (50.8 mm)
  3. 3
    C45 Steel GradeOvakoSteel AISI 1045 · Young's modulus (stiffness): typicalSteel AISI 1045 · Density: typicalSteel AISI 1045 · Poisson's ratio: typicalSteel AISI 1045 · Thermal conductivity: typical range, ambientSteel AISI 1045 · Thermal expansion: typical, mean 20-300 °CSteel AISI 1045 · Specific heat: typical range, 50/100 °C
  4. 4
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 6061-T6 · Poisson's ratio: typical (handbook physical constant)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 6061-T6 stronger than Steel AISI 1045?

Steel AISI 1045 is stronger: its yield strength is 531 MPa against 276 MPa for Aluminum 6061-T6 (1.92x).

Which is lighter, Aluminum 6061-T6 or Steel AISI 1045?

Aluminum 6061-T6 is lighter: 2,700 kg/m³ against 7,800 kg/m³ for Steel AISI 1045.

Which is stiffer, Aluminum 6061-T6 or Steel AISI 1045?

Steel AISI 1045 is stiffer: Young's modulus 210 GPa against 68.3 GPa for Aluminum 6061-T6, so the same part in Steel AISI 1045 deflects less under the same load.

Which is lighter for the same job, Aluminum 6061-T6 or Steel AISI 1045?

For the same stiffness or strength: Aluminum 6061-T6 is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate; Steel AISI 1045 is lighter for a stiff rod or tie (tension).

Part that must beAluminum 6061-T6Steel AISI 1045
Stiff rod or tie (tension)6% heavierlighter
Stiff beam (bending)lighter1.65x heavier
Stiff panel or platelighter1.99x heavier
Strong rod or tielighter1.5x heavier
Strong beamlighter1.87x heavier
Strong panel or platelighter2.08x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 6061-T6 or Steel AISI 1045?

Aluminum 6061-T6 stretches further before it breaks: 17% elongation at break against 12% for Steel AISI 1045.

Thermal

Which conducts heat better, Aluminum 6061-T6 or Steel AISI 1045?

Aluminum 6061-T6 conducts heat better: 167 W/m·K against 42.5 W/m·K for Steel AISI 1045.

Which expands less with temperature?

Steel AISI 1045 expands less: 12 µm/m·K against 23.6 µm/m·K for Aluminum 6061-T6.

Related comparisons