Materials / Compare

Aluminum 7075-T6 vs. FDM Polycarbonate

Compare Aluminum 7075-T6 vs. FDM Polycarbonate strength, stiffness, weight and thermal properties.

Aluminum 7075-T6Wrought
FDM Polycarbonate3D printed (FDM)
MechanicalAluminum 7075-T6FDM Polycarbonate
Yield strength503MPa19.44x stronger53.3MPa2
Ultimate tensile strength572MPa110.7x stronger53.3MPa2
Flexural strengthnot sourced89.4MPa2
Elongation at break11%120% more ductile9.2%2
Young's modulus (stiffness)71GPa129.7x stiffer2.39GPa2
Density2,800kg/m³3range1,180–1,200kg/m³2
Strength to weight180kN·m/kg4.01x higher44.8kN·m/kg
Stiffness to weight25.4MN·m/kg12.6x higher2.01MN·m/kg
Poisson's ratio0.334base material0.385
Shear modulus26.7GPa30.8x stiffer in shear0.867GPa
Bulk modulus69.6GPa20.9x higher3.33GPa
Speed of sound5,036m/s3.55x faster1,418m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6FDM Polycarbonate
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6FDM Polycarbonate
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 7075-T6FDM Polycarbonate
Thermal conductivity130W/m·K3650x more heat through a finbase material0.2W/m·K6
Thermal expansion23.4µm/m·K32.78x lessbase material65µm/m·K6
100 mm part over a 50 °C swing117µm growth2.78x less325µm growth
Specific heat960J/kg·K3not sourced
Heats up and cools (diffusivity)48.4mm²/snot sourced
Thermal shock resistance26,370W/m621x more resistant42.5W/m
Melting pointmelting range532–635°C3not sourced
Glass transitionnot sourced108°C2
Max service temperaturenot sourcedHDT 0.455 MPa105°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6FDM Polycarbonate
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6FDM Polycarbonate
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources6 documents: Kaiser Aluminum, UltiMaker, U.S. Department of Defense, Covestro
Aluminum 7075-T6
7075-T6/T651, Kaiser Aluminum rod & bar (mechanical) and sheet/coil/plate (physical) typical datasheets; Poisson from MIL-HDBK-5J
FDM Polycarbonate
Ultimaker PC, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS (file v5.00), April 20, 2022.
  1. 1
    Alloy 7075 Rod & Bar Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 7075-T6 · Ultimate tensile strength: typicalAluminum 7075-T6 · Elongation at break: typical, in 4DAluminum 7075-T6 · Young's modulus (stiffness): typical
  2. 2
    Ultimaker PC Technical Data Sheet, v5.00UltiMakerarchived copyFDM Polycarbonate · Yield strength: typicalFDM Polycarbonate · Ultimate tensile strength: typical, peak stress (= stress at yield)FDM Polycarbonate · Flexural strength: typicalFDM Polycarbonate · Elongation at break: typicalFDM Polycarbonate · Young's modulus (stiffness): typicalFDM Polycarbonate · Density: rangeFDM Polycarbonate · Glass transition: typicalFDM Polycarbonate · Max service temperature: HDT 0.455 MPa (printed specimens)
  3. 3
    Alloy 7075 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Density: nominalAluminum 7075-T6 · Thermal conductivity: typical, 20 °C, T651Aluminum 7075-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 7075-T6 · Specific heat: typical, at 100 °CAluminum 7075-T6 · Melting point: melting range
  4. 4
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 7075-T6 · Poisson's ratio: typical (handbook physical constant)
  5. 5
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroarchived copyFDM Polycarbonate · Poisson's ratio: base material: polycarbonate family typical (Covestro Part and Mold Design guide, Table 3-1)
  6. 6
    Makrolon 2405 Technical Data SheetCovestroFDM Polycarbonate · Thermal conductivity: base material: Covestro Makrolon 2405 injection-molding PC, typical, through-plane, 23 °CFDM Polycarbonate · Thermal expansion: base material: Covestro Makrolon 2405 injection-molding PC, typical, 23-55 °C, parallel

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

FDM Polycarbonate is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Aluminum 7075-T6 stronger than FDM Polycarbonate?

Aluminum 7075-T6 is stronger: its yield strength is 503 MPa against 53.3 MPa for FDM Polycarbonate (9.44x).

Which is lighter, Aluminum 7075-T6 or FDM Polycarbonate?

FDM Polycarbonate is lighter: 1,190 kg/m³ against 2,800 kg/m³ for Aluminum 7075-T6.

Which is stiffer, Aluminum 7075-T6 or FDM Polycarbonate?

Aluminum 7075-T6 is stiffer: Young's modulus 71 GPa against 2.39 GPa for FDM Polycarbonate, so the same part in Aluminum 7075-T6 deflects less under the same load.

Which is lighter for the same job, Aluminum 7075-T6 or FDM Polycarbonate?

For the same stiffness or strength: Aluminum 7075-T6 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 7075-T6FDM Polycarbonate
Stiff rod or tie (tension)lighter12.6x heavier
Stiff beam (bending)lighter2.31x heavier
Stiff panel or platelighter32% heavier
Strong rod or tielighter4.01x heavier
Strong beamlighter1.9x heavier
Strong panel or platelighter31% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 7075-T6 or FDM Polycarbonate?

Aluminum 7075-T6 stretches further before it breaks: 11% elongation at break against 9.2% for FDM Polycarbonate.

Thermal

Which conducts heat better, Aluminum 7075-T6 or FDM Polycarbonate?

Aluminum 7075-T6 conducts heat better: 130 W/m·K against 0.2 W/m·K for FDM Polycarbonate.

Which expands less with temperature?

Aluminum 7075-T6 expands less: 23.4 µm/m·K against 65 µm/m·K for FDM Polycarbonate.