Materials / Compare

Aluminum 7075-T6 vs. SLS PA12 Nylon

Compare Aluminum 7075-T6 vs. SLS PA12 Nylon strength, stiffness, weight and thermal properties.

Aluminum 7075-T6Wrought
SLS PA12 Nylon3D printed (SLS)
MechanicalAluminum 7075-T6SLS PA12 Nylon
Yield strength503MPa1not given (tensile used)
Ultimate tensile strength572MPa111.9x stronger48MPa2
Elongation at break11%118%21.64x more ductile
Young's modulus (stiffness)71GPa143x stiffer1.65GPa2
Density2,800kg/m³3930kg/m³23.01x lighter
Strength to weight180kN·m/kg3.48x higher51.6kN·m/kg
Stiffness to weight25.4MN·m/kg14.3x higher1.77MN·m/kg
Poisson's ratio0.334not sourced
Shear modulus26.7GPanot sourced
Bulk modulus69.6GPanot sourced
Speed of sound5,036m/s3.78x faster1,332m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000DMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6SLS PA12 Nylon
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ADMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6SLS PA12 Nylon
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 7075-T6SLS PA12 Nylon
Thermal conductivity130W/m·K3not sourced
Thermal expansion23.4µm/m·K3not sourced
100 mm part over a 50 °C swing117µm growthnot sourced
Specific heat960J/kg·K3not sourced
Heats up and cools (diffusivity)48.4mm²/snot sourced
Thermal shock resistance26,370W/mnot sourced
Melting pointmelting range532–635°C3176°C2
Max service temperaturenot sourcedHDT 1.8 MPa64°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 7075-T6
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Kaiser Aluminum, EOS GmbH, U.S. Department of Defense
Aluminum 7075-T6
7075-T6/T651, Kaiser Aluminum rod & bar (mechanical) and sheet/coil/plate (physical) typical datasheets; Poisson from MIL-HDBK-5J
SLS PA12 Nylon
EOS PA 2200 (PA12) Material Data Sheet, process parameter 'Balance' at 120 µm layer thickness, X orientation, dry (conditioned values not given). Live MDS status 04.10.2026, last changed 10.09.2026; PDF via ?topdf=... link on the same page.
  1. 1
    Alloy 7075 Rod & Bar Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 7075-T6 · Ultimate tensile strength: typicalAluminum 7075-T6 · Elongation at break: typical, in 4DAluminum 7075-T6 · Young's modulus (stiffness): typical
  2. 2
    PA 2200 Balance Material Data SheetEOS GmbHSLS PA12 Nylon · Ultimate tensile strength: typicalSLS PA12 Nylon · Elongation at break: typicalSLS PA12 Nylon · Young's modulus (stiffness): typicalSLS PA12 Nylon · Density: typicalSLS PA12 Nylon · Melting point: typicalSLS PA12 Nylon · Max service temperature: HDT 1.8 MPa, X orientation
  3. 3
    Alloy 7075 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Density: nominalAluminum 7075-T6 · Thermal conductivity: typical, 20 °C, T651Aluminum 7075-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 7075-T6 · Specific heat: typical, at 100 °CAluminum 7075-T6 · Melting point: melting range
  4. 4
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 7075-T6 · Poisson's ratio: typical (handbook physical constant)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

SLS PA12 Nylon is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Aluminum 7075-T6 stronger than SLS PA12 Nylon?

Aluminum 7075-T6 is stronger: its yield strength is 503 MPa against tensile strength 48 MPa for SLS PA12 Nylon (10.5x).

Which is lighter, Aluminum 7075-T6 or SLS PA12 Nylon?

SLS PA12 Nylon is lighter: 930 kg/m³ against 2,800 kg/m³ for Aluminum 7075-T6.

Which is stiffer, Aluminum 7075-T6 or SLS PA12 Nylon?

Aluminum 7075-T6 is stiffer: Young's modulus 71 GPa against 1.65 GPa for SLS PA12 Nylon, so the same part in Aluminum 7075-T6 deflects less under the same load.

Which is lighter for the same job, Aluminum 7075-T6 or SLS PA12 Nylon?

For the same stiffness or strength: Aluminum 7075-T6 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 7075-T6SLS PA12 Nylon
Stiff rod or tie (tension)lighter14.3x heavier
Stiff beam (bending)lighter2.18x heavier
Stiff panel or platelighter16% heavier
Strong rod or tielighter3.48x heavier
Strong beamlighter1.59x heavier
Strong panel or platelighter8% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 7075-T6 or SLS PA12 Nylon?

SLS PA12 Nylon stretches further before it breaks: 18% elongation at break against 11% for Aluminum 7075-T6.

Related comparisons