Materials / Compare

Aluminum A380 vs. SLA Resin Standard

Compare Aluminum A380 vs. SLA Resin Standard strength, stiffness, weight and thermal properties.

Aluminum A380Cast
SLA Resin Standard3D printed (SLA resin)
MechanicalAluminum A380SLA Resin Standard
Yield strength160MPa1not given (tensile used)
Ultimate tensile strength320MPa15.33x stronger60MPa2
Flexural strengthnot sourced105MPa2
Elongation at break3.5%18%22.29x more ductile
Young's modulus (stiffness)71GPa125.8x stiffer2.75GPa2
Density2,713kg/m³11,210kg/m³32.24x lighter
Strength to weight59kN·m/kg19% higher49.6kN·m/kg
Stiffness to weight26.2MN·m/kg11.5x higher2.27MN·m/kg
Poisson's ratio0.334not sourced
Shear modulus26.7GPanot sourced
Bulk modulus69.6GPanot sourced
Speed of sound5,116m/s3.39x faster1,508m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum A380SLA Resin Standard
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum A380SLA Resin Standard
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum A380SLA Resin Standard
Thermal conductivity96.2W/m·K1178x more heat through a fin0.54W/m·K5
Thermal expansion21.8µm/m·K15.24x lessmean -30 to 140 °C114µm/m·K5
100 mm part over a 50 °C swing109µm growth5.24x less571µm growth
Specific heat963J/kg·K11,800J/kg·K51.87x higher
Heats up and cools (diffusivity)36.8mm²/s149x faster0.248mm²/s
Thermal shock resistance6,669W/mnot sourced
Max service temperaturenot sourcedHDT 1.8 MPa59°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum A380SLA Resin Standard
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum A380SLA Resin Standard
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: Rheocast Company, Formlabs, North American Die Casting Association
Aluminum A380
A380 aluminium high-pressure die-casting alloy, typical properties; Rheocast Company (aluminium die caster, Germantown WI) A380 alloy data page.
SLA Resin Standard
Formlabs Clear Resin V5 (FLGPCL05), TDS Rev. 01 March 20, 2024; printed on Form 4 at 100 µm, washed 5 min in >=99% IPA, post-cured 15 min at 60 °C in Form Cure. Orientation not stated.
  1. 1
    Alloy Aluminum: A380Rheocast CompanyAluminum A380 · Yield strength: typical, 25 °CAluminum A380 · Ultimate tensile strength: typical, 25 °CAluminum A380 · Elongation at break: typicalAluminum A380 · Young's modulus (stiffness): typical, 25 °CAluminum A380 · Density: typical at 68 °FAluminum A380 · Thermal conductivity: typical at 68 °FAluminum A380 · Thermal expansion: typical, 68-572 °F (20-300 °C)Aluminum A380 · Specific heat: typical at 68 °F
  2. 2
    Clear Resin V5 Technical Data Sheet (2024)Formlabsarchived copySLA Resin Standard · Ultimate tensile strength: typicalSLA Resin Standard · Flexural strength: typicalSLA Resin Standard · Elongation at break: typicalSLA Resin Standard · Young's modulus (stiffness): typicalSLA Resin Standard · Max service temperature: HDT 1.8 MPa
  3. 3
    Clear Resin V5 Technical Data Sheet (web edition)FormlabsSLA Resin Standard · Density: typical, post-cured (same for 5 min ambient and 15 min at 60 °C), ASTM D792
  4. 4
    Product Design for Die Casting, Table 4.1: Die Casting Alloys Material Properties ComparisonNorth American Die Casting Associationarchived copyAluminum A380 · Poisson's ratio: typical, as-cast, separately die cast specimens
  5. 5
    Thermal Properties of Selected Formlabs SLA ResinsFormlabsSLA Resin Standard · Thermal conductivity: typical, post-cured, ASTM E1530SLA Resin Standard · Thermal expansion: mean -30 to 140 °C, post-cured (5 min ambient cure), TMA ASTM E831SLA Resin Standard · Specific heat: typical, 25 °C, post-cured (5 min ambient cure), DSC ASTM E1269

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

SLA Resin Standard is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Aluminum A380 stronger than SLA Resin Standard?

Aluminum A380 is stronger: its yield strength is 160 MPa against tensile strength 60 MPa for SLA Resin Standard (2.67x).

Which is lighter, Aluminum A380 or SLA Resin Standard?

SLA Resin Standard is lighter: 1,210 kg/m³ against 2,713 kg/m³ for Aluminum A380.

Which is stiffer, Aluminum A380 or SLA Resin Standard?

Aluminum A380 is stiffer: Young's modulus 71 GPa against 2.75 GPa for SLA Resin Standard, so the same part in Aluminum A380 deflects less under the same load.

Which is lighter for the same job, Aluminum A380 or SLA Resin Standard?

For the same stiffness or strength: Aluminum A380 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie; SLA Resin Standard is lighter for a strong beam, strong panel or plate.

Part that must beAluminum A380SLA Resin Standard
Stiff rod or tie (tension)lighter11.5x heavier
Stiff beam (bending)lighter2.27x heavier
Stiff panel or platelighter32% heavier
Strong rod or tielighter19% heavier
Strong beam17% heavierlighter
Strong panel or plate37% heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum A380 or SLA Resin Standard?

SLA Resin Standard stretches further before it breaks: 8% elongation at break against 3.5% for Aluminum A380.

Thermal

Which conducts heat better, Aluminum A380 or SLA Resin Standard?

Aluminum A380 conducts heat better: 96.2 W/m·K against 0.54 W/m·K for SLA Resin Standard.

Which expands less with temperature?

Aluminum A380 expands less: 21.8 µm/m·K against 114 µm/m·K for SLA Resin Standard.

Related comparisons