Materials / Compare

Brass C360 vs. FDM HIPS

Compare Brass C360 vs. FDM HIPS strength, stiffness, weight and thermal properties.

Brass C360Wrought
FDM HIPS3D printed (FDM)
MechanicalBrass C360FDM HIPS
Yield strength310MPa1not given (tensile used)
Ultimate tensile strength400MPa121.7x stronger18.4MPa2
Flexural strengthnot sourced31.8MPa2
Elongation at break25%117.9x more ductile1.4%2
Young's modulus (stiffness)96.5GPa160.8x stiffer1.59GPa2
Density8,498kg/m³11,023kg/m³28.31x lighter
Strength to weight36.5kN·m/kg2.03x higher18kN·m/kg
Stiffness to weight11.4MN·m/kg7.32x higher1.55MN·m/kg
Poisson's ratiobase material0.343not sourced
Shear modulus36GPanot sourced
Bulk modulus101GPanot sourced
Speed of sound3,370m/s2.7x faster1,246m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Brass C360FDM HIPS
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Brass C360FDM HIPS
Strength against densityHigher and further left: stronger for its weight
ThermalBrass C360FDM HIPS
Thermal conductivity116W/m·K1682x more heat through a finbase material0.17W/m·K4
Thermal expansion20.5µm/m·K13.9x lessbase material80µm/m·K4
100 mm part over a 50 °C swing103µm growth3.9x less400µm growth
Specific heat377J/kg·K1not sourced
Heats up and cools (diffusivity)36.2mm²/snot sourced
Thermal shock resistance11,997W/mnot sourced
Melting pointsolidus-liquidus888–899°C1not sourced
Glass transitionnot sourced99°C2
Max service temperaturenot sourcedHDT 1.8 MPa86°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Brass C360FDM HIPS
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Brass C360FDM HIPS
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Copper Development Association, BASF Forward AM, Wieland, INEOS Styrolution
Brass C360
C36000 free-cutting brass, H02 half-hard rod 1 in. section (20% cold work), copper.org typical values
FDM HIPS
BASF Forward AM (BASF 3D Printing Solutions) Ultrafuse HiPS, TDS v2.2 (13.11.2019), printed specimens, XY 'Flat'. Specimen print settings are not stated; recommended processing on the sheet: nozzle 240-260 °C, bed 100-120 °C, 40-80 mm/s. Product is discontinued (Forward AM product page) but the TDS is still served by Forward AM.
  1. 1
    C36000 Alloy (copper.org)Copper Development Associationarchived copyBrass C360 · Yield strength: typical, 0.5% extension under loadBrass C360 · Ultimate tensile strength: typicalBrass C360 · Elongation at break: typical, 1 in. rodBrass C360 · Young's modulus (stiffness): typical, temper-independentBrass C360 · Density: nominalBrass C360 · Thermal conductivity: typical, 20 °CBrass C360 · Thermal expansion: typical, mean 20-300 °CBrass C360 · Specific heat: typical, 20 °CBrass C360 · Melting point: solidus-liquidus
  2. 2
    Ultrafuse HiPS Technical Data Sheet, v2.2 (2019)BASF Forward AMarchived copyFDM HIPS · Ultimate tensile strength: typicalFDM HIPS · Flexural strength: typicalFDM HIPS · Elongation at break: typicalFDM HIPS · Young's modulus (stiffness): typicalFDM HIPS · Density: typicalFDM HIPS · Glass transition: typicalFDM HIPS · Max service temperature: HDT 1.8 MPa
  3. 3
    Wieland-Z30 (CuZn39Pb2, C37700) Data SheetWielandarchived copyBrass C360 · Poisson's ratio: base material: leaded free-machining brass CuZn39Pb2 (C37700), Wieland-Z30 rolled products, reference value at room temperature
  4. 4
    Styrolution PS 486N (HIPS) Product Data SheetINEOS StyrolutionFDM HIPS · Thermal conductivity: base material: INEOS Styrolution PS 486N injection-molding HIPS, typicalFDM HIPS · Thermal expansion: base material: INEOS Styrolution PS 486N injection-molding HIPS, typical

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

FDM HIPS is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Brass C360 stronger than FDM HIPS?

Brass C360 is stronger: its yield strength is 310 MPa against tensile strength 18.4 MPa for FDM HIPS (16.8x).

Which is lighter, Brass C360 or FDM HIPS?

FDM HIPS is lighter: 1,023 kg/m³ against 8,498 kg/m³ for Brass C360.

Which is stiffer, Brass C360 or FDM HIPS?

Brass C360 is stiffer: Young's modulus 96.5 GPa against 1.59 GPa for FDM HIPS, so the same part in Brass C360 deflects less under the same load.

Which is lighter for the same job, Brass C360 or FDM HIPS?

For the same stiffness or strength: Brass C360 is lighter for a stiff rod or tie (tension), strong rod or tie; FDM HIPS is lighter for a stiff beam (bending), stiff panel or plate, strong beam, strong panel or plate.

Part that must beBrass C360FDM HIPS
Stiff rod or tie (tension)lighter7.32x heavier
Stiff beam (bending)7% heavierlighter
Stiff panel or plate2.11x heavierlighter
Strong rod or tielighter2.03x heavier
Strong beam26% heavierlighter
Strong panel or plate2.02x heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Brass C360 or FDM HIPS?

Brass C360 stretches further before it breaks: 25% elongation at break against 1.4% for FDM HIPS.

Thermal

Which conducts heat better, Brass C360 or FDM HIPS?

Brass C360 conducts heat better: 116 W/m·K against 0.17 W/m·K for FDM HIPS.

Which expands less with temperature?

Brass C360 expands less: 20.5 µm/m·K against 80 µm/m·K for FDM HIPS.