Materials / Compare

Brass C360 vs. Magnesium AZ31B-H24

Compare Brass C360 vs. Magnesium AZ31B-H24 strength, stiffness, weight and thermal properties.

Brass C360Wrought
Magnesium AZ31B-H24Wrought
MechanicalBrass C360Magnesium AZ31B-H24
Yield strength310MPa141% stronger220MPa2
Ultimate tensile strength400MPa138% stronger290MPa2
Elongation at break25%11.92x more ductile13%2
Young's modulus (stiffness)96.5GPa12.15x stiffer44.8GPa3
Density8,498kg/m³11,769kg/m³34.8x lighter
Strength to weight36.5kN·m/kg124kN·m/kg3.41x higher
Stiffness to weight11.4MN·m/kg25.3MN·m/kg2.23x higher
Poisson's ratiobase material0.3440.353
Shear modulus36GPa2.17x stiffer in shear16.6GPa
Bulk modulus101GPa2.02x higher49.8GPa
Speed of sound3,370m/s5,032m/s49% faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Brass C360Magnesium AZ31B-H24
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Brass C360Magnesium AZ31B-H24
Strength against densityHigher and further left: stronger for its weight
ThermalBrass C360Magnesium AZ31B-H24
Thermal conductivity116W/m·K11.51x more heat through a fin76.9W/m·K2
Thermal expansion20.5µm/m·K131% less26.8µm/m·K2
100 mm part over a 50 °C swing103µm growth31% less134µm growth
Specific heat377J/kg·K11,040J/kg·K22.76x higher
Heats up and cools (diffusivity)36.2mm²/s41.8mm²/s15% faster
Thermal shock resistance11,997W/m31% more resistant9,159W/m
Melting pointsolidus-liquidus888–899°C1not sourced
Max service temperaturenot sourced149°C3
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Brass C360Magnesium AZ31B-H24
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Brass C360Magnesium AZ31B-H24
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Copper Development Association, Magnesium Elektron, U.S. Department of Defense, Wieland
Brass C360
C36000 free-cutting brass, H02 half-hard rod 1 in. section (20% cold work), copper.org typical values
Magnesium AZ31B-H24
AZ31B-H24 sheet 0.016-0.062 in., MIL-HDBK-5J Table 4.2.1.0(b) (AMS 4377); strengths are S-basis MINIMUMS
  1. 1
    C36000 Alloy (copper.org)Copper Development Associationarchived copyBrass C360 · Yield strength: typical, 0.5% extension under loadBrass C360 · Ultimate tensile strength: typicalBrass C360 · Elongation at break: typical, 1 in. rodBrass C360 · Young's modulus (stiffness): typical, temper-independentBrass C360 · Density: nominalBrass C360 · Thermal conductivity: typical, 20 °CBrass C360 · Thermal expansion: typical, mean 20-300 °CBrass C360 · Specific heat: typical, 20 °CBrass C360 · Melting point: solidus-liquidus
  2. 2
    Elektron AZ31B Sheet, Plate & Coil (Datasheet 482)Magnesium Elektronarchived copyMagnesium AZ31B-H24 · Yield strength: typical, H24, 0.5-6 mm, 0.2 % proof stressMagnesium AZ31B-H24 · Ultimate tensile strength: typical, H24, 0.5-6 mmMagnesium AZ31B-H24 · Elongation at break: typical, H24, 0.5-6 mm, gauge 5.65√AMagnesium AZ31B-H24 · Thermal conductivity: typical (temper/temperature not stated)Magnesium AZ31B-H24 · Thermal expansion: typical (temperature range not stated)Magnesium AZ31B-H24 · Specific heat: typical
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseMagnesium AZ31B-H24 · Young's modulus (stiffness): typical (handbook physical constant)Magnesium AZ31B-H24 · Density: nominalMagnesium AZ31B-H24 · Poisson's ratio: typical (handbook physical constant)Magnesium AZ31B-H24 · Max service temperature: stated application limit
  4. 4
    Wieland-Z30 (CuZn39Pb2, C37700) Data SheetWielandarchived copyBrass C360 · Poisson's ratio: base material: leaded free-machining brass CuZn39Pb2 (C37700), Wieland-Z30 rolled products, reference value at room temperature

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Brass C360 stronger than Magnesium AZ31B-H24?

Brass C360 is stronger: its yield strength is 310 MPa against 220 MPa for Magnesium AZ31B-H24 (41%).

Which is lighter, Brass C360 or Magnesium AZ31B-H24?

Magnesium AZ31B-H24 is lighter: 1,769 kg/m³ against 8,498 kg/m³ for Brass C360.

Which is stiffer, Brass C360 or Magnesium AZ31B-H24?

Brass C360 is stiffer: Young's modulus 96.5 GPa against 44.8 GPa for Magnesium AZ31B-H24, so the same part in Brass C360 deflects less under the same load.

Which is lighter for the same job, Brass C360 or Magnesium AZ31B-H24?

For the same stiffness or strength: Magnesium AZ31B-H24 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beBrass C360Magnesium AZ31B-H24
Stiff rod or tie (tension)2.23x heavierlighter
Stiff beam (bending)3.27x heavierlighter
Stiff panel or plate3.72x heavierlighter
Strong rod or tie3.41x heavierlighter
Strong beam3.82x heavierlighter
Strong panel or plate4.05x heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Brass C360 or Magnesium AZ31B-H24?

Brass C360 stretches further before it breaks: 25% elongation at break against 13% for Magnesium AZ31B-H24.

Thermal

Which conducts heat better, Brass C360 or Magnesium AZ31B-H24?

Brass C360 conducts heat better: 116 W/m·K against 76.9 W/m·K for Magnesium AZ31B-H24.

Which expands less with temperature?

Brass C360 expands less: 20.5 µm/m·K against 26.8 µm/m·K for Magnesium AZ31B-H24.

Related comparisons