Materials / Compare
Brass C360 vs. Steel AISI 1045 Compare Brass C360 vs. Steel AISI 1045 strength, stiffness, weight and thermal properties.
Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless Steel 304 Stainless Steel 316 Stainless Steel 303 Stainless Steel 17-4PH Brass C360 Brass C260 Copper C110 Copper C10100 Copper C12200 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Magnesium AZ91D Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall PCB Laminate FR-4 PCB Board FR-4, 2 copper planes Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Solder SAC305 Brass C360 Wrought Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless Steel 304 Stainless Steel 316 Stainless Steel 303 Stainless Steel 17-4PH Brass C360 Brass C260 Copper C110 Copper C10100 Copper C12200 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Magnesium AZ91D Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall PCB Laminate FR-4 PCB Board FR-4, 2 copper planes Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Solder SAC305 Steel AISI 1045 Wrought Mechanical Brass C360 Steel AISI 1045 Yield strength 310 MPa producer-stated 531 MPa 1.71x stronger Ultimate tensile strength 400 MPa producer-stated 627 MPa 1.57x stronger Elongation at break 25 % 2.08x more ductile in 2 in 12 % Young's modulus (stiffness) 96.5 GPa 210 GPa 2.18x stiffer Density 8,498 kg/m³ 7,800 kg/m³ Strength to weight 36.5 kN·m/kg 68.1 kN·m/kg 1.87x higher Stiffness to weight 11.4 MN·m/kg 26.9 MN·m/kg 2.37x higher Poisson's ratio base material 0.34 0.3 Shear modulus 36 GPa 80.8 GPa 2.24x stiffer in shear Bulk modulus 101 GPa 175 GPa 1.74x higher Speed of sound 3,370 m/s 5,189 m/s 1.54x faster
1k 10k 0.1 1 10 100 Density (kg/m³) Young's modulus (GPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Brass C360 Steel AISI 1045 Stiffness against densityHigher and further left: stiffer for its weight 1k 10k 10 100 1k Density (kg/m³) Yield strength (MPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Rubber Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Brick PCB Laminate FR-4 Silicon Ceramic Alumina 96% Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Brass C360 Steel AISI 1045 Strength against densityHigher and further left: stronger for its weight
Thermal Brass C360 Steel AISI 1045 Thermal conductivity 116 W/m·K 40–45 W/m·K Thermal expansion 20.5 µm/m·K 12 µm/m·K 1.71x less 100 mm part over a 50 °C swing 103 µm growth 60 µm growth 1.71x less Specific heat 377 J/kg·K 460–480 J/kg·K Heats up and cools (diffusivity) 36.2 mm²/s 3.12x faster 11.6 mm²/s Thermal shock resistance 11,997 W/m 1.91x more resistant 6,269 W/m Melting point solidus-liquidus 888–899 °C not sourced
1k 10k 0.1 1 10 100 Density (kg/m³) Thermal conductivity (W/m·K) Plastic PLA Plastic PETG Plastic ABS Plastic Nylon Rubber Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM HIPS SLA Resin Standard DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Brass C360 Steel AISI 1045 Thermal conductivity against densityHigher and further left: spreads more heat for its weight 0.1 1 10 100 10 100 Thermal conductivity (W/m·K) Thermal expansion (µm/m·K) Plastic PETG Plastic ABS Plastic Nylon Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM HIPS SLA Resin Standard DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Brass C360 Steel AISI 1045 Thermal expansion against thermal conductivityLower and further right: warps less when heated
Sources 4 documents: Copper Development Association, Niagara LaSalle, Ovako, Wieland
Brass C360 C36000 free-cutting brass, H02 half-hard rod 1 in. section (20% cold work), copper.org typical values
Steel AISI 1045 AISI 1045 cold drawn bar (Niagara LaSalle) for mechanical; Ovako C45 (lists 'SAE 1045' as a similar designation) for physical constants 1 C36000 Alloy (copper.org) Copper Development Association archived copy Brass C360 · Yield strength: typical, 0.5% extension under loadBrass C360 · Ultimate tensile strength: typicalBrass C360 · Elongation at break: typical, 1 in. rodBrass C360 · Young's modulus (stiffness): typical, temper-independentBrass C360 · Density: nominalBrass C360 · Thermal conductivity: typical, 20 °CBrass C360 · Thermal expansion: typical, mean 20-300 °CBrass C360 · Specific heat: typical, 20 °CBrass C360 · Melting point: solidus-liquidus2 1045 Properties Niagara LaSalle archived copy Steel AISI 1045 · Yield strength: producer-stated, cold drawnSteel AISI 1045 · Ultimate tensile strength: producer-stated, cold drawnSteel AISI 1045 · Elongation at break: in 2 in (50.8 mm)3 C45 Steel Grade Ovako Steel AISI 1045 · Young's modulus (stiffness): typicalSteel AISI 1045 · Density: typicalSteel AISI 1045 · Poisson's ratio: typicalSteel AISI 1045 · Thermal conductivity: typical range, ambientSteel AISI 1045 · Thermal expansion: typical, mean 20-300 °CSteel AISI 1045 · Specific heat: typical range, 50/100 °C
4 Wieland-Z30 (CuZn39Pb2, C37700) Data Sheet Wieland archived copy Brass C360 · Poisson's ratio: base material: leaded free-machining brass CuZn39Pb2 (C37700), Wieland-Z30 rolled products, reference value at room temperatureEach number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
Questions Mechanical Is Brass C360 stronger than Steel AISI 1045? Steel AISI 1045 is stronger: its yield strength is 531 MPa against 310 MPa for Brass C360 (1.71x).
Which is lighter, Brass C360 or Steel AISI 1045? Steel AISI 1045 is lighter: 7,800 kg/m³ against 8,498 kg/m³ for Brass C360.
Which is stiffer, Brass C360 or Steel AISI 1045? Steel AISI 1045 is stiffer: Young's modulus 210 GPa against 96.5 GPa for Brass C360, so the same part in Steel AISI 1045 deflects less under the same load.
Which is lighter for the same job, Brass C360 or Steel AISI 1045? For the same stiffness or strength: Steel AISI 1045 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.
Part that must be Brass C360 Steel AISI 1045 Stiff rod or tie (tension) 2.37x heavier lighter Stiff beam (bending) 1.61x heavier lighter Stiff panel or plate 41% heavier lighter Strong rod or tie 1.87x heavier lighter Strong beam 1.56x heavier lighter Strong panel or plate 43% heavier lighter
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Which is more ductile, Brass C360 or Steel AISI 1045? Brass C360 stretches further before it breaks: 25% elongation at break against 12% for Steel AISI 1045.
Thermal Which conducts heat better, Brass C360 or Steel AISI 1045? Brass C360 conducts heat better: 116 W/m·K against 42.5 W/m·K for Steel AISI 1045.
Which expands less with temperature? Steel AISI 1045 expands less: 12 µm/m·K against 20.5 µm/m·K for Brass C360.