Materials / Compare

DMLS 17-4PH Stainless Steel vs. Zinc Zamak 3

Compare DMLS 17-4PH Stainless Steel vs. Zinc Zamak 3 strength, stiffness, weight and thermal properties.

DMLS 17-4PH Stainless Steel3D printed metal (DMLS)
Zinc Zamak 3Cast
MechanicalDMLS 17-4PH Stainless SteelZinc Zamak 3
Yield strengthmean861MPa13.89x stronger221MPa2
Ultimate tensile strengthmean886MPa13.13x stronger283MPa2
Elongation at breakmean at break19.9%11.99x more ductile10%2
Young's modulus (stiffness)base material197GPa32.3x stiffer85.5GPa2
Densitymean part density7,790kg/m³16,600kg/m³218% lighter
Strength to weight110kN·m/kg3.3x higher33.5kN·m/kg
Stiffness to weight25.3MN·m/kg1.95x higher13MN·m/kg
Poisson's ratiobase material0.27230.274
Shear modulus77.4GPa2.3x stiffer in shear33.7GPa
Bulk modulus144GPa2.32x higher62GPa
Speed of sound5,029m/s40% faster3,599m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS 17-4PH Stainless SteelZinc Zamak 3
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS 17-4PH Stainless SteelZinc Zamak 3
Strength against densityHigher and further left: stronger for its weight
ThermalDMLS 17-4PH Stainless SteelZinc Zamak 3
Thermal conductivitybase material17.9W/m·K3113W/m·K26.31x more heat through a fin
Thermal expansionmean 25-100 °C10.4µm/m·K12.63x less27.4µm/m·K2
100 mm part over a 50 °C swing52µm growth2.63x less137µm growth
Specific heatbase material460J/kg·K3419J/kg·K2
Heats up and cools (diffusivity)5mm²/s40.9mm²/s8.19x faster
Thermal shock resistance5,474W/m7,782W/m42% more resistant
Melting pointnot sourcedmelting range381–387°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS 17-4PH Stainless SteelZinc Zamak 3
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS 17-4PH Stainless SteelZinc Zamak 3
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: EOS GmbH, Nathan Trotter, Cleveland-Cliffs, Eastern Alloys
DMLS 17-4PH Stainless Steel
EOS StainlessSteel 17-4PH IndustryLine (powder 9011-0041), EOS M 290, 40 µm, default job 17-4PH_040_StainlessM291_100, as built, horizontal; ISO 6892 & ASTM E8M
Zinc Zamak 3
Zamak 3 (ASTM B86 die cast), Nathan Trotter (zinc alloy producer) technical data sheet, typical values
  1. 1
    EOS StainlessSteel 17-4PH IndustryLine Material Data Sheet, M 290EOS GmbHarchived copyDMLS 17-4PH Stainless Steel · Yield strength: mean, as built, horizontal (N=72)DMLS 17-4PH Stainless Steel · Ultimate tensile strength: mean, as built, horizontal (N=72)DMLS 17-4PH Stainless Steel · Elongation at break: mean at break, as built, horizontalDMLS 17-4PH Stainless Steel · Density: mean part density (ISO 3369)DMLS 17-4PH Stainless Steel · Thermal expansion: mean 25-100 °C, ASTM E228, AFTER atmospheric heat treatment (as-built value not published)
  2. 2
    Zamak 3 Technical Data SheetNathan Trotterarchived copyZinc Zamak 3 · Yield strength: typicalZinc Zamak 3 · Ultimate tensile strength: typicalZinc Zamak 3 · Elongation at break: typical, in 2 in.Zinc Zamak 3 · Young's modulus (stiffness): typicalZinc Zamak 3 · Density: typicalZinc Zamak 3 · Thermal conductivity: typicalZinc Zamak 3 · Thermal expansion: typicalZinc Zamak 3 · Specific heat: typicalZinc Zamak 3 · Melting point: melting range
  3. 3
    17-4 PH Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsDMLS 17-4PH Stainless Steel · Young's modulus (stiffness): base material: wrought 17-4 PH, Condition H 900 (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Poisson's ratio: base material: wrought 17-4 PH, all conditions (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Thermal conductivity: base material: wrought 17-4 PH, Condition H 900, at 149 °C (Cleveland-Cliffs)DMLS 17-4PH Stainless Steel · Specific heat: base material: wrought 17-4 PH, Condition A, 0-100 °C (Cleveland-Cliffs)
  4. 4
    Zinc Die Casting Properties Guide (2012)Eastern AlloysZinc Zamak 3 · Poisson's ratio: typical, Zamak 3 hot-chamber die cast

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

DMLS 17-4PH Stainless Steel is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is DMLS 17-4PH Stainless Steel stronger than Zinc Zamak 3?

DMLS 17-4PH Stainless Steel is stronger: its yield strength is 861 MPa against 221 MPa for Zinc Zamak 3 (3.89x).

Which is lighter, DMLS 17-4PH Stainless Steel or Zinc Zamak 3?

Zinc Zamak 3 is lighter: 6,600 kg/m³ against 7,790 kg/m³ for DMLS 17-4PH Stainless Steel.

Which is stiffer, DMLS 17-4PH Stainless Steel or Zinc Zamak 3?

DMLS 17-4PH Stainless Steel is stiffer: Young's modulus 197 GPa against 85.5 GPa for Zinc Zamak 3, so the same part in DMLS 17-4PH Stainless Steel deflects less under the same load.

Which is lighter for the same job, DMLS 17-4PH Stainless Steel or Zinc Zamak 3?

For the same stiffness or strength: DMLS 17-4PH Stainless Steel is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beDMLS 17-4PH Stainless SteelZinc Zamak 3
Stiff rod or tie (tension)lighter1.95x heavier
Stiff beam (bending)lighter29% heavier
Stiff panel or platelighter12% heavier
Strong rod or tielighter3.3x heavier
Strong beamlighter2.1x heavier
Strong panel or platelighter1.67x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, DMLS 17-4PH Stainless Steel or Zinc Zamak 3?

DMLS 17-4PH Stainless Steel stretches further before it breaks: 19.9% elongation at break against 10% for Zinc Zamak 3.

Thermal

Which conducts heat better, DMLS 17-4PH Stainless Steel or Zinc Zamak 3?

Zinc Zamak 3 conducts heat better: 113 W/m·K against 17.9 W/m·K for DMLS 17-4PH Stainless Steel.

Which expands less with temperature?

DMLS 17-4PH Stainless Steel expands less: 10.4 µm/m·K against 27.4 µm/m·K for Zinc Zamak 3.

Related comparisons