Materials / Compare

DMLS AlSi10Mg Aluminum vs. FDM PAHT-CF

Compare DMLS AlSi10Mg Aluminum vs. FDM PAHT-CF strength, stiffness, weight and thermal properties.

DMLS AlSi10Mg Aluminum3D printed metal (DMLS)
FDM PAHT-CF3D printed (FDM)
MechanicalDMLS AlSi10Mg AluminumFDM PAHT-CF
Yield strength270MPa1not given (tensile used)
Ultimate tensile strength450MPa14.89x stronger92MPa2
Flexural strengthnot sourced125MPa2
Elongation at break10.2%121% more ductile8.4%2
Young's modulus (stiffness)72GPa318.7x stiffer3.86GPa2
Density2,670kg/m³41,060kg/m³22.52x lighter
Strength to weight101kN·m/kg17% higher86.8kN·m/kg
Stiffness to weight27MN·m/kg7.41x higher3.64MN·m/kg
Poisson's ratiobase material0.335not sourced
Shear modulus27.1GPanot sourced
Bulk modulus70.6GPanot sourced
Speed of sound5,193m/s2.72x faster1,908m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumFDM PAHT-CF
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg AluminumFDM PAHT-CF
Strength against densityHigher and further left: stronger for its weight
ThermalDMLS AlSi10Mg AluminumFDM PAHT-CF
Thermal conductivity110W/m·K1not sourced
Thermal expansionmean 25-100 °C20µm/m·K1not sourced
100 mm part over a 50 °C swing100µm growthnot sourced
Specific heatbase material963J/kg·K5not sourced
Heats up and cools (diffusivity)42.8mm²/snot sourced
Thermal shock resistance13,819W/mnot sourced
Melting pointnot sourced225°C2
Glass transitionnot sourced70°C2
Max service temperaturenot sourcedHDT 1.8 MPa170°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg Aluminum
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS AlSi10Mg Aluminum
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: EOS GmbH, Bambu Lab, Renishaw, U.S. Department of Defense
DMLS AlSi10Mg Aluminum
EOS Aluminium AlSi10Mg (powder 9011-0024), EOS M 290 | 30 µm process (AlSi10Mg_FlexM291 2.01), as manufactured, horizontal; machined (turned) specimens, ISO 6892-1 B10
FDM PAHT-CF
Bambu Lab PAHT-CF, TDS V3.0, printed specimens X-Y, dry state; nozzle 290 °C, bed 100 °C, 100 mm/s, 100% infill; annealed and dried 80 °C for 12 h before testing.
  1. 1
    EOS Aluminium AlSi10Mg Material Data SheetEOS GmbHarchived copyDMLS AlSi10Mg Aluminum · Yield strength: typical, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Ultimate tensile strength: typical, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Elongation at break: typical at break, as manufactured, horizontalDMLS AlSi10Mg Aluminum · Thermal conductivity: typical, as manufactured, horizontal (ISO 22007-2)DMLS AlSi10Mg Aluminum · Thermal expansion: mean 25-100 °C, ASTM E228
  2. 2
    Bambu PAHT-CF Technical Data Sheet, V3.0Bambu LabFDM PAHT-CF · Ultimate tensile strength: typicalFDM PAHT-CF · Flexural strength: typicalFDM PAHT-CF · Elongation at break: typicalFDM PAHT-CF · Young's modulus (stiffness): typicalFDM PAHT-CF · Density: typicalFDM PAHT-CF · Melting point: typicalFDM PAHT-CF · Glass transition: typicalFDM PAHT-CF · Max service temperature: HDT 1.8 MPa
  3. 3
    RenAM 500 Series Aluminium AlSi10Mg Material Data SheetRenishawDMLS AlSi10Mg Aluminum · Young's modulus (stiffness): same material and process, different machine maker: Renishaw RenAM 500, 30 µm, as built, horizontal (XY)
  4. 4
    EOS Aluminium AlSi10Mg Material Data Sheet, FlexLine, M 290 (2018)EOS GmbHarchived copyDMLS AlSi10Mg Aluminum · Density: typical part density (ISO 3369), EOS M 290, AlSi10Mg_030_FlexM291 (30 µm)
  5. 5
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseDMLS AlSi10Mg Aluminum · Poisson's ratio: base material: cast Al-Si-Mg alloy 359.0 (Al-9Si-0.6Mg, closest MIL-HDBK-5J alloy to AlSi10Mg / EN AC-43000)DMLS AlSi10Mg Aluminum · Specific heat: base material: cast Al-Si-Mg alloy 359.0 (MIL-HDBK-5J), at 100 °C

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

DMLS AlSi10Mg Aluminum and FDM PAHT-CF are 3D printed: their properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is DMLS AlSi10Mg Aluminum stronger than FDM PAHT-CF?

DMLS AlSi10Mg Aluminum is stronger: its yield strength is 270 MPa against tensile strength 92 MPa for FDM PAHT-CF (2.93x).

Which is lighter, DMLS AlSi10Mg Aluminum or FDM PAHT-CF?

FDM PAHT-CF is lighter: 1,060 kg/m³ against 2,670 kg/m³ for DMLS AlSi10Mg Aluminum.

Which is stiffer, DMLS AlSi10Mg Aluminum or FDM PAHT-CF?

DMLS AlSi10Mg Aluminum is stiffer: Young's modulus 72 GPa against 3.86 GPa for FDM PAHT-CF, so the same part in DMLS AlSi10Mg Aluminum deflects less under the same load.

Which is lighter for the same job, DMLS AlSi10Mg Aluminum or FDM PAHT-CF?

For the same stiffness or strength: DMLS AlSi10Mg Aluminum is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie; FDM PAHT-CF is lighter for a strong beam, strong panel or plate.

Part that must beDMLS AlSi10Mg AluminumFDM PAHT-CF
Stiff rod or tie (tension)lighter7.41x heavier
Stiff beam (bending)lighter1.71x heavier
Stiff panel or platelighter5% heavier
Strong rod or tielighter17% heavier
Strong beam23% heavierlighter
Strong panel or plate47% heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, DMLS AlSi10Mg Aluminum or FDM PAHT-CF?

DMLS AlSi10Mg Aluminum stretches further before it breaks: 10.2% elongation at break against 8.4% for FDM PAHT-CF.

Related comparisons