Materials / Compare

DMLS Ti-6Al-4V ELI Titanium vs. FDM Polycarbonate

Compare DMLS Ti-6Al-4V ELI Titanium vs. FDM Polycarbonate strength, stiffness, weight and thermal properties.

DMLS Ti-6Al-4V ELI Titanium3D printed metal (DMLS)
FDM Polycarbonate3D printed (FDM)
MechanicalDMLS Ti-6Al-4V ELI TitaniumFDM Polycarbonate
Yield strength1,100MPa120.6x stronger53.3MPa2
Ultimate tensile strength1,270MPa123.8x stronger53.3MPa2
Flexural strengthnot sourced89.4MPa2
Elongation at break8.7%19.2%2
Young's modulus (stiffness)same maker and process110GPa345.9x stiffer2.39GPa2
Density4,400kg/m³1range1,180–1,200kg/m³2
Strength to weight250kN·m/kg5.58x higher44.8kN·m/kg
Stiffness to weight25MN·m/kg12.4x higher2.01MN·m/kg
Poisson's ratiowrought TIMETAL 6-40.3424base material0.385
Shear modulus41GPa47.2x stiffer in shear0.867GPa
Bulk modulus116GPa34.9x higher3.33GPa
Speed of sound5,000m/s3.53x faster1,418m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS Ti-6Al-4V ELI TitaniumFDM Polycarbonate
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS Ti-6Al-4V ELI TitaniumFDM Polycarbonate
Strength against densityHigher and further left: stronger for its weight
ThermalDMLS Ti-6Al-4V ELI TitaniumFDM Polycarbonate
Thermal conductivitybase material6.6W/m·K633x more heat through a finbase material0.2W/m·K7
Thermal expansionmean 25-100 °C9µm/m·K87.22x lessbase material65µm/m·K7
100 mm part over a 50 °C swing45µm growth7.22x less325µm growth
Specific heatbase material580J/kg·K6not sourced
Heats up and cools (diffusivity)2.59mm²/snot sourced
Thermal shock resistance4,825W/m114x more resistant42.5W/m
Melting pointmelting range1,630–1,650°C4not sourced
Glass transitionnot sourced108°C2
Max service temperaturenot sourcedHDT 0.455 MPa105°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS Ti-6Al-4V ELI TitaniumFDM Polycarbonate
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS Ti-6Al-4V ELI TitaniumFDM Polycarbonate
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources8 documents: EOS GmbH, UltiMaker, TIMET, Covestro
DMLS Ti-6Al-4V ELI Titanium
EOS Titanium Ti64ELI (powder 9011-0040; ASTM F136/F3001, i.e. Grade 23) on EOS M400 SF, parameter set Ti64ELI_030_FlexM400_100, 30 µm, as built; ISO 6892-1 A14
FDM Polycarbonate
Ultimaker PC, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS (file v5.00), April 20, 2022.
  1. 1
    EOS Titanium Ti64ELI Material Data Sheet, M 290 and M 400EOS GmbHarchived copyDMLS Ti-6Al-4V ELI Titanium · Yield strength: typical, as built, average of horizontal + vertical (M400)DMLS Ti-6Al-4V ELI Titanium · Ultimate tensile strength: typical, as built, average of horizontal + vertical (M400)DMLS Ti-6Al-4V ELI Titanium · Elongation at break: typical at break, as built (M400)DMLS Ti-6Al-4V ELI Titanium · Density: typical part density (ISO 3369), M400
  2. 2
    Ultimaker PC Technical Data Sheet, v5.00UltiMakerarchived copyFDM Polycarbonate · Yield strength: typicalFDM Polycarbonate · Ultimate tensile strength: typical, peak stress (= stress at yield)FDM Polycarbonate · Flexural strength: typicalFDM Polycarbonate · Elongation at break: typicalFDM Polycarbonate · Young's modulus (stiffness): typicalFDM Polycarbonate · Density: rangeFDM Polycarbonate · Glass transition: typicalFDM Polycarbonate · Max service temperature: HDT 0.455 MPa (printed specimens)
  3. 3
    EOS Titanium Ti64 Material Data Sheet, M 290 (2022)EOS GmbHarchived copyDMLS Ti-6Al-4V ELI Titanium · Young's modulus (stiffness): same maker and process, sibling grade: EOS Titanium Ti64 (Grade 5) on EOS M 290, as built, XY and Z, typical
  4. 4
    TIMETAL 6-4 PropertiesTIMETarchived copyDMLS Ti-6Al-4V ELI Titanium · Poisson's ratio: wrought TIMETAL 6-4 (TIMET measurement, mean of 10); composition-level, not DMLS-measuredDMLS Ti-6Al-4V ELI Titanium · Melting point: melting range, wrought TIMETAL 6-4 (composition-level)
  5. 5
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroarchived copyFDM Polycarbonate · Poisson's ratio: base material: polycarbonate family typical (Covestro Part and Mold Design guide, Table 3-1)
  6. 6
    TIMETAL 6-4 Data SheetTIMETarchived copyDMLS Ti-6Al-4V ELI Titanium · Thermal conductivity: base material: wrought Ti-6Al-4V / 6-4 ELI (TIMET datasheet), 20 °CDMLS Ti-6Al-4V ELI Titanium · Specific heat: base material: wrought Ti-6Al-4V / 6-4 ELI (TIMET datasheet), 20 °C
  7. 7
    Makrolon 2405 Technical Data SheetCovestroFDM Polycarbonate · Thermal conductivity: base material: Covestro Makrolon 2405 injection-molding PC, typical, through-plane, 23 °CFDM Polycarbonate · Thermal expansion: base material: Covestro Makrolon 2405 injection-molding PC, typical, 23-55 °C, parallel
  8. 8
    EOS Titanium Ti64 Grade 23 Material Data SheetEOS GmbHarchived copyDMLS Ti-6Al-4V ELI Titanium · Thermal expansion: mean 25-100 °C, ASTM E228; EOS Ti64 Grade 23 (=ELI) on EOS M 290 40 µm; condition not stated (sheet's mechanical data are heat treated)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

DMLS Ti-6Al-4V ELI Titanium and FDM Polycarbonate are 3D printed: their properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is DMLS Ti-6Al-4V ELI Titanium stronger than FDM Polycarbonate?

DMLS Ti-6Al-4V ELI Titanium is stronger: its yield strength is 1,100 MPa against 53.3 MPa for FDM Polycarbonate (20.6x).

Which is lighter, DMLS Ti-6Al-4V ELI Titanium or FDM Polycarbonate?

FDM Polycarbonate is lighter: 1,190 kg/m³ against 4,400 kg/m³ for DMLS Ti-6Al-4V ELI Titanium.

Which is stiffer, DMLS Ti-6Al-4V ELI Titanium or FDM Polycarbonate?

DMLS Ti-6Al-4V ELI Titanium is stiffer: Young's modulus 110 GPa against 2.39 GPa for FDM Polycarbonate, so the same part in DMLS Ti-6Al-4V ELI Titanium deflects less under the same load.

Which is lighter for the same job, DMLS Ti-6Al-4V ELI Titanium or FDM Polycarbonate?

For the same stiffness or strength: DMLS Ti-6Al-4V ELI Titanium is lighter for a stiff rod or tie (tension), stiff beam (bending), strong rod or tie, strong beam, strong panel or plate; FDM Polycarbonate is lighter for a stiff panel or plate.

Part that must beDMLS Ti-6Al-4V ELI TitaniumFDM Polycarbonate
Stiff rod or tie (tension)lighter12.4x heavier
Stiff beam (bending)lighter1.83x heavier
Stiff panel or plate3% heavierlighter
Strong rod or tielighter5.58x heavier
Strong beamlighter2.03x heavier
Strong panel or platelighter23% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Thermal

Which conducts heat better, DMLS Ti-6Al-4V ELI Titanium or FDM Polycarbonate?

DMLS Ti-6Al-4V ELI Titanium conducts heat better: 6.6 W/m·K against 0.2 W/m·K for FDM Polycarbonate.

Which expands less with temperature?

DMLS Ti-6Al-4V ELI Titanium expands less: 9 µm/m·K against 65 µm/m·K for FDM Polycarbonate.