Materials / Compare

FDM HIPS vs. Plastic POM/Acetal

Compare FDM HIPS vs. Plastic POM/Acetal strength, stiffness, weight and thermal properties.

FDM HIPS3D printed (FDM)
Plastic POM/AcetalBulk polymer (molded or machined)
MechanicalFDM HIPSPlastic POM/Acetal
Yield strengthnot given (tensile used)69MPa1
Ultimate tensile strength18.4MPa269MPa13.75x stronger
Compressive strengthnot sourced124MPa1
Flexural strength31.8MPa299MPa1
Elongation at break1.4%275%153.6x more ductile
Young's modulus (stiffness)1.59GPa22.8GPa11.76x stiffer
Density1,023kg/m³239% lighter1,420kg/m³3
Strength to weight18kN·m/kg48.6kN·m/kg2.7x higher
Stiffness to weight1.55MN·m/kg1.97MN·m/kg27% higher
Poisson's rationot sourced0.351
Shear modulusnot sourced1.04GPa
Bulk modulusnot sourced3.11GPa
Speed of sound1,246m/s1,404m/s13% faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM HIPSPlastic POM/Acetal
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM HIPSPlastic POM/Acetal
Strength against densityHigher and further left: stronger for its weight
ThermalFDM HIPSPlastic POM/Acetal
Thermal conductivitybase material0.17W/m·K40.4W/m·K12.35x more heat through a fin
Thermal expansionbase material80µm/m·K41.52x lessmean122µm/m·K1
100 mm part over a 50 °C swing400µm growth1.52x less610µm growth
Specific heatnot sourcedaverage -18 to 100 °C1,465J/kg·K1
Heats up and cools (diffusivity)not sourced0.192mm²/s
Thermal shock resistancenot sourced52.5W/m
Melting pointnot sourced175°C1
Glass transition99°C2not sourced
Max service temperatureHDT 1.8 MPa86°C2HDT 1.8 MPa125°C139 °C hotter
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM HIPSPlastic POM/Acetal
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM HIPSPlastic POM/Acetal
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: DuPont, BASF Forward AM, INEOS Styrolution
FDM HIPS
BASF Forward AM (BASF 3D Printing Solutions) Ultrafuse HiPS, TDS v2.2 (13.11.2019), printed specimens, XY 'Flat'. Specimen print settings are not stated; recommended processing on the sheet: nozzle 240-260 °C, bed 100-120 °C, 40-80 mm/s. Product is discontinued (Forward AM product page) but the TDS is still served by Forward AM.
Plastic POM/Acetal
DuPont Delrin 100 acetal homopolymer, Table 2 'Typical Properties of Delrin Acetal Resins' (ASTM methods), Delrin Design Guide Module III hosted on delrin.com
  1. 1
    Delrin Acetal Resin Design Guide, Module IIIDuPontarchived copyPlastic POM/Acetal · Yield strength: typical (single ASTM D638 tensile strength)Plastic POM/Acetal · Ultimate tensile strength: typicalPlastic POM/Acetal · Compressive strength: compressive stress at 10% deformationPlastic POM/Acetal · Flexural strength: flexural yield strength, typicalPlastic POM/Acetal · Elongation at break: typicalPlastic POM/Acetal · Young's modulus (stiffness): typicalPlastic POM/Acetal · Poisson's ratio: typicalPlastic POM/Acetal · Thermal conductivity: typicalPlastic POM/Acetal · Thermal expansion: mean, 29 to 60 °CPlastic POM/Acetal · Specific heat: average -18 to 100 °C, Delrin acetal resins (not grade-specific)Plastic POM/Acetal · Melting point: crystalline melting pointPlastic POM/Acetal · Max service temperature: HDT 1.8 MPa (annealed)
  2. 2
    Ultrafuse HiPS Technical Data Sheet, v2.2 (2019)BASF Forward AMarchived copyFDM HIPS · Ultimate tensile strength: typicalFDM HIPS · Flexural strength: typicalFDM HIPS · Elongation at break: typicalFDM HIPS · Young's modulus (stiffness): typicalFDM HIPS · Density: typicalFDM HIPS · Glass transition: typicalFDM HIPS · Max service temperature: HDT 1.8 MPa
  3. 3
    Delrin 100 Product Data SheetDuPontPlastic POM/Acetal · Density: typical (DuPont product information for Delrin 100 NC010; 'The data listed here fall within the normal range of product properties')
  4. 4
    Styrolution PS 486N (HIPS) Product Data SheetINEOS StyrolutionFDM HIPS · Thermal conductivity: base material: INEOS Styrolution PS 486N injection-molding HIPS, typicalFDM HIPS · Thermal expansion: base material: INEOS Styrolution PS 486N injection-molding HIPS, typical

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

FDM HIPS is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is FDM HIPS stronger than Plastic POM/Acetal?

Plastic POM/Acetal is stronger: its yield strength is 69 MPa against tensile strength 18.4 MPa for FDM HIPS (3.75x).

Which is lighter, FDM HIPS or Plastic POM/Acetal?

FDM HIPS is lighter: 1,023 kg/m³ against 1,420 kg/m³ for Plastic POM/Acetal.

Which is stiffer, FDM HIPS or Plastic POM/Acetal?

Plastic POM/Acetal is stiffer: Young's modulus 2.8 GPa against 1.59 GPa for FDM HIPS, so the same part in Plastic POM/Acetal deflects less under the same load.

Which is lighter for the same job, FDM HIPS or Plastic POM/Acetal?

For the same stiffness or strength: FDM HIPS is lighter for a stiff beam (bending), stiff panel or plate; Plastic POM/Acetal is lighter for a stiff rod or tie (tension), strong rod or tie, strong beam, strong panel or plate.

Part that must beFDM HIPSPlastic POM/Acetal
Stiff rod or tie (tension)27% heavierlighter
Stiff beam (bending)lighter5% heavier
Stiff panel or platelighter15% heavier
Strong rod or tie2.7x heavierlighter
Strong beam1.74x heavierlighter
Strong panel or plate40% heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, FDM HIPS or Plastic POM/Acetal?

Plastic POM/Acetal stretches further before it breaks: 75% elongation at break against 1.4% for FDM HIPS.

Thermal

Which handles higher temperatures, FDM HIPS or Plastic POM/Acetal?

Plastic POM/Acetal does: 125 °C against 86 °C for FDM HIPS.

Which conducts heat better, FDM HIPS or Plastic POM/Acetal?

Plastic POM/Acetal conducts heat better: 0.4 W/m·K against 0.17 W/m·K for FDM HIPS.

Which expands less with temperature?

FDM HIPS expands less: 80 µm/m·K against 122 µm/m·K for Plastic POM/Acetal.

Related comparisons