| Mechanical | ||
| Yield strength | not given (tensile used) | 885MPasourcetypical, plate (>0.187 in), annealed, 0.2% offset |
| Ultimate tensile strength | 18.4MPasourcetypical | 940MPasourcetypical, plate, annealed |
| Flexural strength | 31.8MPasourcetypical | not sourced |
| Elongation at break | 1.4%sourcetypical | 16%sourcetypical, in 2 in., plate annealed |
| Young's modulus (stiffness) | 1.59GPasourcetypical | 107–122GPasourcetypical range, 20 °C |
| Density | 1,023kg/m³sourcetypical | 4,430kg/m³sourcenominal |
| Strength to weight | 18kN·m/kg | 200kN·m/kg11.1x higher |
| Stiffness to weight | 1.55MN·m/kg | 25.8MN·m/kg16.7x higher |
| Poisson's ratio | not sourced | 0.342sourcemean of TIMET measurements |
| Shear modulus | not sourced | 42.7GPa |
| Bulk modulus | not sourced | 121GPa |
| Speed of sound | 1,246m/s | 5,084m/s |
| Thermal | ||
| Thermal conductivity | 0.17W/m·Ksourcebase material: INEOS Styrolution PS 486N injection-molding HIPS, typical | 6.6W/m·Ksourcetypical, 20 °C, mill annealed |
| Thermal expansion | 80µm/m·Ksourcebase material: INEOS Styrolution PS 486N injection-molding HIPS, typical | 9µm/m·Ksourcetypical, mean 0-100 °C |
| 100 mm part over a 50 °C swing | 400µm growth | 45µm growth8.89x less |
| Specific heat | not sourced | 580J/kg·Ksourcetypical, 20 °C |
| Heats up and cools (diffusivity) | not sourced | 2.57mm²/s |
| Thermal shock resistance | not sourced | 3,730W/m |
| Melting point | not sourced | 1,630–1,650°Csourcemelting range |
| Glass transition | 99°Csourcetypical | not sourced |
| Max service temperature | 86°CsourceHDT 1.8 MPa | 400°Csourceupper recommended use temperature |
| Values for | BASF Forward AM (BASF 3D Printing Solutions) Ultrafuse HiPS, TDS v2.2 (13.11.2019), printed specimens, XY 'Flat'. Specimen print settings are not stated; recommended processing on the sheet: nozzle 240-260 °C, bed 100-120 °C, 40-80 mm/s. Product is discontinued (Forward AM product page) but the TDS is still served by Forward AM. | TIMETAL 6-4 (Ti-6Al-4V Grade 5) annealed plate typical (TIMET properties manual) + TIMET datasheet TMC-0150 physical properties |
Every value links to the document that states it. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
FDM HIPS is 3D printed: its properties depend on build direction and print settings; these are typical values.
Questions
Is FDM HIPS stronger than Titanium Ti-6Al-4V?
Titanium Ti-6Al-4V is stronger: its yield strength is 885 MPa against tensile strength 18.4 MPa for FDM HIPS (48.1x).
Which is lighter, FDM HIPS or Titanium Ti-6Al-4V?
FDM HIPS is lighter: 1,023 kg/m³ against 4,430 kg/m³ for Titanium Ti-6Al-4V.
Which is stiffer, FDM HIPS or Titanium Ti-6Al-4V?
Titanium Ti-6Al-4V is stiffer: Young's modulus 115 GPa against 1.59 GPa for FDM HIPS, so the same part in Titanium Ti-6Al-4V deflects less under the same load.
Which is lighter for the same job, FDM HIPS or Titanium Ti-6Al-4V?
For the same stiffness or strength: FDM HIPS is lighter for a stiff panel or plate; Titanium Ti-6Al-4V is lighter for a stiff rod or tie (tension), stiff beam (bending), strong rod or tie, strong beam, strong panel or plate.
| Part that must be | FDM HIPS | Titanium Ti-6Al-4V |
|---|---|---|
| Stiff rod or tie (tension) | 16.7x heavier | lighter |
| Stiff beam (bending) | 1.96x heavier | lighter |
| Stiff panel or plate | lighter | 4% heavier |
| Strong rod or tie | 11.1x heavier | lighter |
| Strong beam | 3.05x heavier | lighter |
| Strong panel or plate | 1.6x heavier | lighter |
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Which conducts heat better, FDM HIPS or Titanium Ti-6Al-4V?
Titanium Ti-6Al-4V conducts heat better: 6.6 W/m·K against 0.17 W/m·K for FDM HIPS.
Which expands less with temperature?
Titanium Ti-6Al-4V expands less: 9 µm/m·K against 80 µm/m·K for FDM HIPS.