Materials / Compare

Magnesium AZ31B-H24 vs. Stainless Steel 17-4PH

Compare Magnesium AZ31B-H24 vs. Stainless Steel 17-4PH strength, stiffness, weight and thermal properties.

Magnesium AZ31B-H24Wrought
Stainless Steel 17-4PHWrought
MechanicalMagnesium AZ31B-H24Stainless Steel 17-4PH
Yield strength220MPa11,275MPa25.8x stronger
Ultimate tensile strength290MPa11,379MPa24.76x stronger
Elongation at break13%144% more ductile9%2
Young's modulus (stiffness)44.8GPa3H 900197GPa24.4x stiffer
Density1,769kg/m³34.41x lighterH 9007,800kg/m³2
Strength to weight124kN·m/kg163kN·m/kg31% higher
Stiffness to weight25.3MN·m/kg25.3MN·m/kg
Poisson's ratio0.353H 9000.2722
Shear modulus16.6GPa77.4GPa4.67x stiffer in shear
Bulk modulus49.8GPa144GPa2.89x higher
Speed of sound5,032m/s5,026m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Stainless Steel 17-4PH
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Stainless Steel 17-4PH
Strength against densityHigher and further left: stronger for its weight
ThermalMagnesium AZ31B-H24Stainless Steel 17-4PH
Thermal conductivity76.9W/m·K14.3x more heat through a finat 149 °C17.9W/m·K2
Thermal expansion26.8µm/m·K1mean10.8µm/m·K22.48x less
100 mm part over a 50 °C swing134µm growth54µm growth2.48x less
Specific heat1,040J/kg·K12.26x highermean460J/kg·K2
Heats up and cools (diffusivity)41.8mm²/s8.38x faster4.99mm²/s
Thermal shock resistance9,159W/m17% more resistant7,809W/m
Max service temperature149°C3316°C2167 °C hotter
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Stainless Steel 17-4PH
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Aluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Stainless Steel 17-4PH
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources3 documents: Magnesium Elektron, Cleveland-Cliffs, U.S. Department of Defense
Magnesium AZ31B-H24
AZ31B-H24 sheet 0.016-0.062 in., MIL-HDBK-5J Table 4.2.1.0(b) (AMS 4377); strengths are S-basis MINIMUMS
Stainless Steel 17-4PH
Cleveland-Cliffs 17-4 PH, Condition H 900, sheet/strip, transverse (Product Data Bulletin, May 2021)
  1. 1
    Elektron AZ31B Sheet, Plate & Coil (Datasheet 482)Magnesium Elektronarchived copyMagnesium AZ31B-H24 · Yield strength: typical, H24, 0.5-6 mm, 0.2 % proof stressMagnesium AZ31B-H24 · Ultimate tensile strength: typical, H24, 0.5-6 mmMagnesium AZ31B-H24 · Elongation at break: typical, H24, 0.5-6 mm, gauge 5.65√AMagnesium AZ31B-H24 · Thermal conductivity: typical (temper/temperature not stated)Magnesium AZ31B-H24 · Thermal expansion: typical (temperature range not stated)Magnesium AZ31B-H24 · Specific heat: typical
  2. 2
    17-4 PH Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsStainless Steel 17-4PH · Yield strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Ultimate tensile strength: typical, transverse, sheet/stripStainless Steel 17-4PH · Elongation at break: typical, transverse, in 2 in. (50.8 mm)Stainless Steel 17-4PH · Young's modulus (stiffness): H 900Stainless Steel 17-4PH · Density: H 900Stainless Steel 17-4PH · Poisson's ratio: H 900 (column)Stainless Steel 17-4PH · Thermal conductivity: at 149 °C (300 °F), H 900Stainless Steel 17-4PH · Thermal expansion: mean, 21–93 °C (70–200 °F), H 900Stainless Steel 17-4PH · Specific heat: mean, 0–100 °C, H 900Stainless Steel 17-4PH · Max service temperature: strength-retention limit (not oxidation)
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseMagnesium AZ31B-H24 · Young's modulus (stiffness): typical (handbook physical constant)Magnesium AZ31B-H24 · Density: nominalMagnesium AZ31B-H24 · Poisson's ratio: typical (handbook physical constant)Magnesium AZ31B-H24 · Max service temperature: stated application limit

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Magnesium AZ31B-H24 stronger than Stainless Steel 17-4PH?

Stainless Steel 17-4PH is stronger: its yield strength is 1,275 MPa against 220 MPa for Magnesium AZ31B-H24 (5.8x).

Which is lighter, Magnesium AZ31B-H24 or Stainless Steel 17-4PH?

Magnesium AZ31B-H24 is lighter: 1,769 kg/m³ against 7,800 kg/m³ for Stainless Steel 17-4PH.

Which is stiffer, Magnesium AZ31B-H24 or Stainless Steel 17-4PH?

Stainless Steel 17-4PH is stiffer: Young's modulus 197 GPa against 44.8 GPa for Magnesium AZ31B-H24, so the same part in Stainless Steel 17-4PH deflects less under the same load.

Which is lighter for the same job, Magnesium AZ31B-H24 or Stainless Steel 17-4PH?

For the same stiffness or strength: Magnesium AZ31B-H24 is lighter for a stiff beam (bending), stiff panel or plate, strong beam, strong panel or plate; Stainless Steel 17-4PH is lighter for a strong rod or tie.

Part that must beMagnesium AZ31B-H24Stainless Steel 17-4PH
Stiff rod or tie (tension)about equalabout equal
Stiff beam (bending)lighter2.1x heavier
Stiff panel or platelighter2.69x heavier
Strong rod or tie31% heavierlighter
Strong beamlighter37% heavier
Strong panel or platelighter1.83x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Magnesium AZ31B-H24 or Stainless Steel 17-4PH?

Magnesium AZ31B-H24 stretches further before it breaks: 13% elongation at break against 9% for Stainless Steel 17-4PH.

Thermal

Which handles higher temperatures, Magnesium AZ31B-H24 or Stainless Steel 17-4PH?

Stainless Steel 17-4PH does: 316 °C against 149 °C for Magnesium AZ31B-H24.

Which conducts heat better, Magnesium AZ31B-H24 or Stainless Steel 17-4PH?

Magnesium AZ31B-H24 conducts heat better: 76.9 W/m·K against 17.9 W/m·K for Stainless Steel 17-4PH.

Which expands less with temperature?

Stainless Steel 17-4PH expands less: 10.8 µm/m·K against 26.8 µm/m·K for Magnesium AZ31B-H24.