Materials / Compare

Magnesium AZ31B-H24 vs. Steel

Compare Magnesium AZ31B-H24 vs. Steel strength, stiffness, weight and thermal properties.

Magnesium AZ31B-H24Wrought
SteelWrought
MechanicalMagnesium AZ31B-H24Steel
Yield strength220MPa1385MPa21.75x stronger
Ultimate tensile strength290MPa1505MPa21.74x stronger
Elongation at break13%124.2%21.86x more ductile
Young's modulus (stiffness)44.8GPa3design value200GPa4
Density1,769kg/m³34.44x lighter7,850kg/m³5
Strength to weight124kN·m/kg2.54x higher49kN·m/kg
Stiffness to weight25.3MN·m/kg25.5MN·m/kg
Poisson's ratio0.353design value0.34
Shear modulus16.6GPa76.9GPa4.64x stiffer in shear
Bulk modulus49.8GPa167GPa3.35x higher
Speed of sound5,032m/s5,048m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Steel
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Steel
Strength against densityHigher and further left: stronger for its weight
ThermalMagnesium AZ31B-H24Steel
Thermal conductivity76.9W/m·K11.6x more heat through a fin48W/m·K5
Thermal expansion26.8µm/m·K112µm/m·K52.23x less
100 mm part over a 50 °C swing134µm growth60µm growth2.23x less
Specific heat1,040J/kg·K1base material460–480J/kg·K6
Heats up and cools (diffusivity)41.8mm²/s3.21x faster13mm²/s
Thermal shock resistance9,159W/m1.7x more resistant5,390W/m
Max service temperature149°C3not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Steel
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Magnesium AZ31B-H24Steel
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources6 documents: Magnesium Elektron, American Institute of Steel Construction, U.S. Department of Defense, bauforumstahl (ArcelorMittal), Ovako
Magnesium AZ31B-H24
AZ31B-H24 sheet 0.016-0.062 in., MIL-HDBK-5J Table 4.2.1.0(b) (AMS 4377); strengths are S-basis MINIMUMS
Steel
Generic structural steel, cited as ASTM A992 (the current US structural grade): ASTM A992 W-shapes; Fy/Fu specified minimums from AISC publications (AISC 360-16 Commentary; Modern Steel Construction); elastic constants AISC 360; physical constants from the bauforumstahl structural-steel EPD, which names A992 among covered product standards.
  1. 1
    Elektron AZ31B Sheet, Plate & Coil (Datasheet 482)Magnesium Elektronarchived copyMagnesium AZ31B-H24 · Yield strength: typical, H24, 0.5-6 mm, 0.2 % proof stressMagnesium AZ31B-H24 · Ultimate tensile strength: typical, H24, 0.5-6 mmMagnesium AZ31B-H24 · Elongation at break: typical, H24, 0.5-6 mm, gauge 5.65√AMagnesium AZ31B-H24 · Thermal conductivity: typical (temper/temperature not stated)Magnesium AZ31B-H24 · Thermal expansion: typical (temperature range not stated)Magnesium AZ31B-H24 · Specific heat: typical
  2. 2
    Updating Standard Shape Material Properties Database for Design and ReliabilityAmerican Institute of Steel Constructionarchived copySteel · Yield strength: typical: mean of 20,295 A992 flange mill-test coupons (1998 SSPC survey), as reported by AISCSteel · Ultimate tensile strength: typical: mean of 20,295 A992 flange mill-test coupons (1998 SSPC survey)Steel · Elongation at break: typical: mean of 24,847 A992 mill-test elongations, web and flange (1998 SSPC mill data), as reported by AISC
  3. 3
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseMagnesium AZ31B-H24 · Young's modulus (stiffness): typical (handbook physical constant)Magnesium AZ31B-H24 · Density: nominalMagnesium AZ31B-H24 · Poisson's ratio: typical (handbook physical constant)Magnesium AZ31B-H24 · Max service temperature: stated application limit
  4. 4
    ANSI/AISC 360-16 Specification for Structural Steel Buildings, with CommentaryAmerican Institute of Steel Constructionarchived copySteel · Young's modulus (stiffness): design value (AISC 360-16)Steel · Poisson's ratio: design value (AISC 360-16 Commentary)
  5. 5
    Environmental Product Declaration: Structural Steel Sections and Merchant Bars (2023)bauforumstahl (ArcelorMittal)archived copySteel · Density: nominal (constructional data)Steel · Thermal conductivity: nominal at 20 °CSteel · Thermal expansion: nominal (constructional data, no temperature range stated)
  6. 6
    S275JR Steel GradeOvakoSteel · Specific heat: base material: EN S275JR unalloyed structural steel (the EN counterpart of A36), typical, 50/100 °C

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Magnesium AZ31B-H24 stronger than Steel?

Steel is stronger: its yield strength is 385 MPa against 220 MPa for Magnesium AZ31B-H24 (1.75x).

Which is lighter, Magnesium AZ31B-H24 or Steel?

Magnesium AZ31B-H24 is lighter: 1,769 kg/m³ against 7,850 kg/m³ for Steel.

Which is stiffer, Magnesium AZ31B-H24 or Steel?

Steel is stiffer: Young's modulus 200 GPa against 44.8 GPa for Magnesium AZ31B-H24, so the same part in Steel deflects less under the same load.

Which is lighter for the same job, Magnesium AZ31B-H24 or Steel?

For the same stiffness or strength: Magnesium AZ31B-H24 is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.

Part that must beMagnesium AZ31B-H24Steel
Stiff rod or tie (tension)about equalabout equal
Stiff beam (bending)lighter2.1x heavier
Stiff panel or platelighter2.69x heavier
Strong rod or tielighter2.54x heavier
Strong beamlighter3.06x heavier
Strong panel or platelighter3.35x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Magnesium AZ31B-H24 or Steel?

Steel stretches further before it breaks: 24.2% elongation at break against 13% for Magnesium AZ31B-H24.

Thermal

Which conducts heat better, Magnesium AZ31B-H24 or Steel?

Magnesium AZ31B-H24 conducts heat better: 76.9 W/m·K against 48 W/m·K for Steel.

Which expands less with temperature?

Steel expands less: 12 µm/m·K against 26.8 µm/m·K for Magnesium AZ31B-H24.