Materials / Compare
Magnesium AZ31B-H24 vs. Zinc Zamak 3 Compare Magnesium AZ31B-H24 vs. Zinc Zamak 3 strength, stiffness, weight and thermal properties.
Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless Steel 304 Stainless Steel 316 Stainless Steel 303 Stainless Steel 17-4PH Brass C360 Brass C260 Copper C110 Copper C10100 Copper C12200 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Magnesium AZ91D Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall PCB Laminate FR-4 PCB Board FR-4, 2 copper planes Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Solder SAC305 Magnesium AZ31B-H24 Wrought Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Rubber Wood Aluminum Aluminum 6061-T6 Aluminum 7075-T6 Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Steel Steel AISI 1018 Steel AISI 1045 Steel AISI 4340 Steel A992 Iron Titanium Titanium Ti-6Al-4V Stainless Steel 304 Stainless Steel 316 Stainless Steel 303 Stainless Steel 17-4PH Brass C360 Brass C260 Copper C110 Copper C10100 Copper C12200 Glass Nickel Inconel 718 Magnesium AZ31B-H24 Magnesium AZ91D Zinc Zamak 3 FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood Drywall PCB Laminate FR-4 PCB Board FR-4, 2 copper planes Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Solder SAC305 Zinc Zamak 3 Cast Mechanical Magnesium AZ31B-H24 Zinc Zamak 3 Yield strength 220 MPa 221 MPa Ultimate tensile strength 290 MPa 283 MPa Elongation at break 13 % 30% more ductile 10 % Young's modulus (stiffness) 44.8 GPa 85.5 GPa 1.91x stiffer Density 1,769 kg/m³ 3.73x lighter 6,600 kg/m³ Strength to weight 124 kN·m/kg 3.71x higher 33.5 kN·m/kg Stiffness to weight 25.3 MN·m/kg 1.95x higher 13 MN·m/kg Poisson's ratio 0.35 0.27 Shear modulus 16.6 GPa 33.7 GPa 2.03x stiffer in shear Bulk modulus 49.8 GPa 62 GPa 24% higher Speed of sound 5,032 m/s 40% faster 3,599 m/s
1k 10k 0.1 1 10 100 Density (kg/m³) Young's modulus (GPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Magnesium AZ31B-H24 Zinc Zamak 3 Stiffness against densityHigher and further left: stiffer for its weight 1k 10k 10 100 1k Density (kg/m³) Yield strength (MPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Rubber Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Brick PCB Laminate FR-4 Silicon Ceramic Alumina 96% Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Magnesium AZ31B-H24 Zinc Zamak 3 Strength against densityHigher and further left: stronger for its weight
Thermal Magnesium AZ31B-H24 Zinc Zamak 3 Thermal conductivity 76.9 W/m·K 113 W/m·K 47% more heat through a fin Thermal expansion 26.8 µm/m·K 27.4 µm/m·K 100 mm part over a 50 °C swing 134 µm growth 2% less 137 µm growth Specific heat 1,040 J/kg·K 2.48x higher 419 J/kg·K Heats up and cools (diffusivity) 41.8 mm²/s 2% faster 40.9 mm²/s Thermal shock resistance 9,159 W/m 18% more resistant 7,782 W/m Melting point not sourced melting range 381–387 °C Max service temperature 149 °C not sourced
1k 10k 0.1 1 10 100 Density (kg/m³) Thermal conductivity (W/m·K) Plastic PLA Plastic PETG Plastic ABS Plastic Nylon Rubber Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM HIPS SLA Resin Standard DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Magnesium AZ31B-H24 Zinc Zamak 3 Thermal conductivity against densityHigher and further left: spreads more heat for its weight 0.1 1 10 100 10 100 Thermal conductivity (W/m·K) Thermal expansion (µm/m·K) Plastic PETG Plastic ABS Plastic Nylon Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM HIPS SLA Resin Standard DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum A380 Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Magnesium AZ31B-H24 Zinc Zamak 3 Thermal expansion against thermal conductivityLower and further right: warps less when heated
Sources 4 documents: Magnesium Elektron, Nathan Trotter, U.S. Department of Defense, Eastern Alloys
Magnesium AZ31B-H24 AZ31B-H24 sheet 0.016-0.062 in., MIL-HDBK-5J Table 4.2.1.0(b) (AMS 4377); strengths are S-basis MINIMUMS
Zinc Zamak 3 Zamak 3 (ASTM B86 die cast), Nathan Trotter (zinc alloy producer) technical data sheet, typical values 1 Elektron AZ31B Sheet, Plate & Coil (Datasheet 482) Magnesium Elektron archived copy Magnesium AZ31B-H24 · Yield strength: typical, H24, 0.5-6 mm, 0.2 % proof stressMagnesium AZ31B-H24 · Ultimate tensile strength: typical, H24, 0.5-6 mmMagnesium AZ31B-H24 · Elongation at break: typical, H24, 0.5-6 mm, gauge 5.65√AMagnesium AZ31B-H24 · Thermal conductivity: typical (temper/temperature not stated)Magnesium AZ31B-H24 · Thermal expansion: typical (temperature range not stated)Magnesium AZ31B-H24 · Specific heat: typical2 Zamak 3 Technical Data Sheet Nathan Trotter archived copy Zinc Zamak 3 · Yield strength: typicalZinc Zamak 3 · Ultimate tensile strength: typicalZinc Zamak 3 · Elongation at break: typical, in 2 in.Zinc Zamak 3 · Young's modulus (stiffness): typicalZinc Zamak 3 · Density: typicalZinc Zamak 3 · Thermal conductivity: typicalZinc Zamak 3 · Thermal expansion: typicalZinc Zamak 3 · Specific heat: typicalZinc Zamak 3 · Melting point: melting range3 MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003) U.S. Department of Defense Magnesium AZ31B-H24 · Young's modulus (stiffness): typical (handbook physical constant)Magnesium AZ31B-H24 · Density: nominalMagnesium AZ31B-H24 · Poisson's ratio: typical (handbook physical constant)Magnesium AZ31B-H24 · Max service temperature: stated application limit
4 Zinc Die Casting Properties Guide (2012) Eastern Alloys Zinc Zamak 3 · Poisson's ratio: typical, Zamak 3 hot-chamber die cast
Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.
Questions Mechanical Is Magnesium AZ31B-H24 stronger than Zinc Zamak 3? Zinc Zamak 3 is stronger: its yield strength is 221 MPa against 220 MPa for Magnesium AZ31B-H24 (0%).
Which is lighter, Magnesium AZ31B-H24 or Zinc Zamak 3? Magnesium AZ31B-H24 is lighter: 1,769 kg/m³ against 6,600 kg/m³ for Zinc Zamak 3.
Which is stiffer, Magnesium AZ31B-H24 or Zinc Zamak 3? Zinc Zamak 3 is stiffer: Young's modulus 85.5 GPa against 44.8 GPa for Magnesium AZ31B-H24, so the same part in Zinc Zamak 3 deflects less under the same load.
Which is lighter for the same job, Magnesium AZ31B-H24 or Zinc Zamak 3? For the same stiffness or strength: Magnesium AZ31B-H24 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate.
Part that must be Magnesium AZ31B-H24 Zinc Zamak 3 Stiff rod or tie (tension) lighter 1.95x heavier Stiff beam (bending) lighter 2.7x heavier Stiff panel or plate lighter 3.01x heavier Strong rod or tie lighter 3.71x heavier Strong beam lighter 3.72x heavier Strong panel or plate lighter 3.72x heavier
For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).
Which is more ductile, Magnesium AZ31B-H24 or Zinc Zamak 3? Magnesium AZ31B-H24 stretches further before it breaks: 13% elongation at break against 10% for Zinc Zamak 3.
Thermal Which conducts heat better, Magnesium AZ31B-H24 or Zinc Zamak 3? Zinc Zamak 3 conducts heat better: 113 W/m·K against 76.9 W/m·K for Magnesium AZ31B-H24.
Which expands less with temperature? Magnesium AZ31B-H24 expands less: 26.8 µm/m·K against 27.4 µm/m·K for Zinc Zamak 3.