Materials / Compare

Plastic ABS vs. Zinc Zamak 3

Compare Plastic ABS vs. Zinc Zamak 3 strength, stiffness, weight and thermal properties.

Plastic ABS3D printed (FDM)
Zinc Zamak 3Cast
MechanicalPlastic ABSZinc Zamak 3
Yield strength38.1MPa1221MPa25.8x stronger
Ultimate tensile strength38.1MPa1283MPa27.43x stronger
Flexural strength61.1MPa1not sourced
Elongation at break4.6%110%22.17x more ductile
Young's modulus (stiffness)1.96GPa185.5GPa243.6x stiffer
Density1,100kg/m³16x lighter6,600kg/m³2
Strength to weight34.6kN·m/kg3% higher33.5kN·m/kg
Stiffness to weight1.78MN·m/kg13MN·m/kg7.26x higher
Poisson's ratiobase material0.3930.274
Shear modulus0.706GPa33.7GPa47.7x stiffer in shear
Bulk modulus2.97GPa62GPa20.8x higher
Speed of sound1,336m/s3,599m/s2.69x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic ABSZinc Zamak 3
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic ABSZinc Zamak 3
Strength against densityHigher and further left: stronger for its weight
ThermalPlastic ABSZinc Zamak 3
Thermal conductivitybase material0.17W/m·K5113W/m·K2665x more heat through a fin
Thermal expansionbase material80–110µm/m·K527.4µm/m·K2
100 mm part over a 50 °C swing475µm growth137µm growth3.47x less
Specific heatnot sourced419J/kg·K2
Heats up and cools (diffusivity)not sourced40.9mm²/s
Thermal shock resistance21.2W/m7,782W/m367x more resistant
Melting pointnot sourcedmelting range381–387°C2
Glass transition101°C1not sourced
Max service temperatureHDT 0.455 MPa86.6°C1not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic ABSZinc Zamak 3
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic ABSZinc Zamak 3
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: UltiMaker, Nathan Trotter, Covestro, Eastern Alloys, INEOS Styrolution
Plastic ABS
Ultimaker ABS, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS v5.00, April 20, 2022.
Zinc Zamak 3
Zamak 3 (ASTM B86 die cast), Nathan Trotter (zinc alloy producer) technical data sheet, typical values
  1. 1
    Ultimaker ABS Technical Data Sheet, v5.00UltiMakerarchived copyPlastic ABS · Yield strength: typicalPlastic ABS · Ultimate tensile strength: typical, peak stress (= stress at yield)Plastic ABS · Flexural strength: typicalPlastic ABS · Elongation at break: typicalPlastic ABS · Young's modulus (stiffness): typicalPlastic ABS · Density: typicalPlastic ABS · Glass transition: typicalPlastic ABS · Max service temperature: HDT 0.455 MPa (printed specimens)
  2. 2
    Zamak 3 Technical Data SheetNathan Trotterarchived copyZinc Zamak 3 · Yield strength: typicalZinc Zamak 3 · Ultimate tensile strength: typicalZinc Zamak 3 · Elongation at break: typical, in 2 in.Zinc Zamak 3 · Young's modulus (stiffness): typicalZinc Zamak 3 · Density: typicalZinc Zamak 3 · Thermal conductivity: typicalZinc Zamak 3 · Thermal expansion: typicalZinc Zamak 3 · Specific heat: typicalZinc Zamak 3 · Melting point: melting range
  3. 3
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroarchived copyPlastic ABS · Poisson's ratio: base material: ABS family typical (Covestro Part and Mold Design guide, Table 3-1)
  4. 4
    Zinc Die Casting Properties Guide (2012)Eastern AlloysZinc Zamak 3 · Poisson's ratio: typical, Zamak 3 hot-chamber die cast
  5. 5
    Terluran GP-22 (ABS) Product Data SheetINEOS StyrolutionPlastic ABS · Thermal conductivity: base material: INEOS Styrolution Terluran GP-22 injection-molding ABS, typicalPlastic ABS · Thermal expansion: base material: INEOS Styrolution Terluran GP-22 injection-molding ABS, range

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Plastic ABS is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is Plastic ABS stronger than Zinc Zamak 3?

Zinc Zamak 3 is stronger: its yield strength is 221 MPa against 38.1 MPa for Plastic ABS (5.8x).

Which is lighter, Plastic ABS or Zinc Zamak 3?

Plastic ABS is lighter: 1,100 kg/m³ against 6,600 kg/m³ for Zinc Zamak 3.

Which is stiffer, Plastic ABS or Zinc Zamak 3?

Zinc Zamak 3 is stiffer: Young's modulus 85.5 GPa against 1.96 GPa for Plastic ABS, so the same part in Zinc Zamak 3 deflects less under the same load.

Which is lighter for the same job, Plastic ABS or Zinc Zamak 3?

For the same stiffness or strength: Plastic ABS is lighter for a stiff panel or plate, strong rod or tie, strong beam, strong panel or plate; Zinc Zamak 3 is lighter for a stiff rod or tie (tension), stiff beam (bending).

Part that must bePlastic ABSZinc Zamak 3
Stiff rod or tie (tension)7.26x heavierlighter
Stiff beam (bending)10% heavierlighter
Stiff panel or platelighter1.71x heavier
Strong rod or tielighter3% heavier
Strong beamlighter1.86x heavier
Strong panel or platelighter2.49x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Plastic ABS or Zinc Zamak 3?

Zinc Zamak 3 stretches further before it breaks: 10% elongation at break against 4.6% for Plastic ABS.

Thermal

Which conducts heat better, Plastic ABS or Zinc Zamak 3?

Zinc Zamak 3 conducts heat better: 113 W/m·K against 0.17 W/m·K for Plastic ABS.

Which expands less with temperature?

Zinc Zamak 3 expands less: 27.4 µm/m·K against 95 µm/m·K for Plastic ABS.

Related comparisons