Materials / Compare

Plastic PBT GF30 vs. Steel

Compare Plastic PBT GF30 vs. Steel strength, stiffness, weight and thermal properties.

Plastic PBT GF30Bulk polymer (molded or machined)
SteelWrought
MechanicalPlastic PBT GF30Steel
Yield strengthnot given (tensile used)385MPa1
Ultimate tensile strengthstress at break140MPa2505MPa1
Flexural strength210MPa2not sourced
Elongation at breakstrain at break3%224.2%18.07x more ductile
Young's modulus (stiffness)9.8GPa2design value200GPa3
Density1,530kg/m³25.13x lighter7,850kg/m³4
Strength to weight91.5kN·m/kg1.87x higher49kN·m/kg
Stiffness to weight6.41MN·m/kg25.5MN·m/kg3.98x higher
Poisson's rationot sourceddesign value0.33
Shear modulusnot sourced76.9GPa
Bulk modulusnot sourced167GPa
Speed of sound2,531m/s5,048m/s1.99x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PPS GF40Plastic LCP GF30Plastic PBT GF30Steel
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PPS GF40Plastic LCP GF30Plastic PBT GF30Steel
Strength against densityHigher and further left: stronger for its weight
ThermalPlastic PBT GF30Steel
Thermal conductivity0.27W/m·K248W/m·K4178x more heat through a fin
Thermal expansionlongitudinal25µm/m·K212µm/m·K42.08x less
100 mm part over a 50 °C swing125µm growth60µm growth2.08x less
Specific heat1,050J/kg·K2base material460–480J/kg·K5
Heats up and cools (diffusivity)0.168mm²/s13mm²/s77.4x faster
Thermal shock resistancenot sourced5,390W/m
Melting pointDSC223°C2not sourced
Max service temperatureHDT 1.8 MPa205°C2not sourced
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PPS GF40Plastic LCP GF30Plastic PBT GF30Steel
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PPS GF40Plastic LCP GF30Plastic PBT GF30Steel
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources5 documents: American Institute of Steel Construction, BASF, bauforumstahl (ArcelorMittal), Ovako
Plastic PBT GF30
BASF Ultradur B 4300 G6 (PBT, 30% glass fibre), injection moulding grade; product information sheet 09/2026, typical values for uncoloured product at 23 °C.
Steel
Generic structural steel, cited as ASTM A992 (the current US structural grade): ASTM A992 W-shapes; Fy/Fu specified minimums from AISC publications (AISC 360-16 Commentary; Modern Steel Construction); elastic constants AISC 360; physical constants from the bauforumstahl structural-steel EPD, which names A992 among covered product standards.
  1. 1
    Updating Standard Shape Material Properties Database for Design and ReliabilityAmerican Institute of Steel Constructionarchived copySteel · Yield strength: typical: mean of 20,295 A992 flange mill-test coupons (1998 SSPC survey), as reported by AISCSteel · Ultimate tensile strength: typical: mean of 20,295 A992 flange mill-test coupons (1998 SSPC survey)Steel · Elongation at break: typical: mean of 24,847 A992 mill-test elongations, web and flange (1998 SSPC mill data), as reported by AISC
  2. 2
    Ultradur B 4300 G6 Product InformationBASFPlastic PBT GF30 · Ultimate tensile strength: stress at break, 23 °CPlastic PBT GF30 · Flexural strength: typical, 23 °CPlastic PBT GF30 · Elongation at break: strain at break, 23 °CPlastic PBT GF30 · Young's modulus (stiffness): typical, 23 °CPlastic PBT GF30 · Density: typicalPlastic PBT GF30 · Thermal conductivity: typical (DIN 52612-1)Plastic PBT GF30 · Thermal expansion: longitudinal (flow), mean 23-55 °CPlastic PBT GF30 · Specific heat: typical, 23 °CPlastic PBT GF30 · Melting point: DSC (ISO 11357)Plastic PBT GF30 · Max service temperature: HDT 1.8 MPa
  3. 3
    ANSI/AISC 360-16 Specification for Structural Steel Buildings, with CommentaryAmerican Institute of Steel Constructionarchived copySteel · Young's modulus (stiffness): design value (AISC 360-16)Steel · Poisson's ratio: design value (AISC 360-16 Commentary)
  4. 4
    Environmental Product Declaration: Structural Steel Sections and Merchant Bars (2023)bauforumstahl (ArcelorMittal)archived copySteel · Density: nominal (constructional data)Steel · Thermal conductivity: nominal at 20 °CSteel · Thermal expansion: nominal (constructional data, no temperature range stated)
  5. 5
    S275JR Steel GradeOvakoSteel · Specific heat: base material: EN S275JR unalloyed structural steel (the EN counterpart of A36), typical, 50/100 °C

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Plastic PBT GF30 stronger than Steel?

Steel is stronger: its yield strength is 385 MPa against tensile strength 140 MPa for Plastic PBT GF30 (2.75x).

Which is lighter, Plastic PBT GF30 or Steel?

Plastic PBT GF30 is lighter: 1,530 kg/m³ against 7,850 kg/m³ for Steel.

Which is stiffer, Plastic PBT GF30 or Steel?

Steel is stiffer: Young's modulus 200 GPa against 9.8 GPa for Plastic PBT GF30, so the same part in Steel deflects less under the same load.

Which is lighter for the same job, Plastic PBT GF30 or Steel?

For the same stiffness or strength: Plastic PBT GF30 is lighter for a stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam, strong panel or plate; Steel is lighter for a stiff rod or tie (tension).

Part that must bePlastic PBT GF30Steel
Stiff rod or tie (tension)3.98x heavierlighter
Stiff beam (bending)lighter14% heavier
Stiff panel or platelighter1.88x heavier
Strong rod or tielighter1.87x heavier
Strong beamlighter2.61x heavier
Strong panel or platelighter3.09x heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Plastic PBT GF30 or Steel?

Steel stretches further before it breaks: 24.2% elongation at break against 3% for Plastic PBT GF30.

Thermal

Which conducts heat better, Plastic PBT GF30 or Steel?

Steel conducts heat better: 48 W/m·K against 0.27 W/m·K for Plastic PBT GF30.

Which expands less with temperature?

Steel expands less: 12 µm/m·K against 25 µm/m·K for Plastic PBT GF30.